WELDER QUALIFICATION REQUIERMENT

120 views
Skip to first unread message

QA/QC

unread,
Jul 14, 2022, 3:48:57 AM7/14/22
to Materials & Welding
Dear Experts

i have two wps's for piping cs/ltsc welding with the asme b31.3 ans sec 9  one thickness range is 3 to 20 mm and the second is 20.01to 31.22  pwht requiered .the two is GTAW+SMAW

i have a welder qualify in test coupon 6'' 14.27 mm 

my question is this welder will qualify to weld in the two wps or we should make another qualification for him seperately 

Vishwas Keskar

unread,
Jul 14, 2022, 4:02:24 AM7/14/22
to material...@googlegroups.com
Welder qualification range is independent of thickness  range of WPS s.

What is his weld metal deposition qualification
GTAW ___mm??
SMAW __mm??



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/083762d2-dd64-482a-85e9-0e4f7aa4e14bn%40googlegroups.com.

james gerald

unread,
Jul 14, 2022, 4:28:54 AM7/14/22
to material...@googlegroups.com
Please see snapshot of ASME Sec.IX.

Inline image


Thanks & Regards

J.Gerald Jayakumar




Adnan Ziad

unread,
Jul 14, 2022, 5:17:36 AM7/14/22
to material...@googlegroups.com

Vishwas Keskar

unread,
Jul 14, 2022, 5:38:16 AM7/14/22
to material...@googlegroups.com
So he is qualified  for  weld deposit in production Welding for 

GTAW = 10mm maximum
SMAW=18.54 mm maximum

The essential variables of WPS, WPQ shall be  checked and followed during production Welding.



james gerald

unread,
Jul 14, 2022, 7:09:51 AM7/14/22
to material...@googlegroups.com
What you have mentioned is Basemetal thickness but in Welder qualification only weld metal thickness is an essential variable qualified from 0 to applicable weld metal thickness for each process, BM thickness is unlimited

Thanks & Regards

J.Gerald Jayakumar


On Thursday, 14 July, 2022 at 01:18:52 pm IST, QA/QC <adnan...@gmail.com> wrote:


Adnan Ziad

unread,
Jul 14, 2022, 7:39:46 AM7/14/22
to material...@googlegroups.com
In our case he weld 5 mm gtaw + 9.27 mm smaw 

Can i qualify him directly on the two wps 

james gerald

unread,
Jul 14, 2022, 7:48:07 AM7/14/22
to material...@googlegroups.com
Choose a higher thickness pipe say 20mm wherein you can weld GTAW 5mm (2t) and SMAW 15mm with minimum 3 layers so for SMAW he will be qualified for unlimited thickness and say GTAW 10mm/

Thanks & Regards

J.Gerald Jayakumar