Hardness range for CS+ Alloy0625 clad welding

75 views
Skip to first unread message

Saurabh Jain

unread,
Aug 18, 2025, 10:17:46 PMAug 18
to material...@googlegroups.com
Dear experts.

I am currently in the process of qualifying a PQR for API 5L X65 + A350 LF6. Both material consists of a base metal with alloy 0625 cladding. Welding process: GTAW+SMAW

During the mechanical testing, I witnessed the following hardness values:
Clad material: 300 to 390 HV
Weld metal: 280 to 350 HV

This is for Aramco project, so I referred their standard 01-SAMSS-044, and it specifies that I must refer to NACE MR0175/ISO 15156 for hardness acceptance criteria, particularly for the clad.

I have reviewed the standard but cannot find a specific acceptable hardness range. I also checked Aramco's W-11/W-12 and W-16 standards but was unable to find the maximum allowable hardness for clad welding.

My question is: Are these recorded hardness values for the clad and weld metal acceptable under the NACE MR0175/ISO 15156 standard? If not, what are the typical hardness limitations and under which standard?

Regards 
Saurabh Jain

Mohmmed Dudhiyawala

unread,
Oct 17, 2025, 1:26:35 AMOct 17
to Materials & Welding
Dear Saurabh,
Refer Table A.12 of NACE MR0175/ISO 15156, where Inconel 625 is designated as Type 4d.
Refer Table A.14. From Temp<149°C, Inconel 625 can be used for all conditions, stipulated in table. Hardness to be limited to 40 HRC max. (392 HV).


Regards,
Mohammed

Saurabh Jain

unread,
Oct 17, 2025, 2:18:52 AMOct 17
to material...@googlegroups.com
Dear Mohammed,

Thank you for your response.

We're facing another significant issue.

Most of our carbon steel Procedure Qualification Records covering groups G1-G2, G1-G3 & G2-G3, G3-G3 with various process combinations are showing an unacceptable hardness range (260–325 HV) in the Heat-Affected Zone.

Our maximum acceptable hardness limit is 250 HV.

We've used different testing agencies, yet the results remain consistently high.


Regards,

Saurabh


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/a43d8910-6d95-4287-be8b-e6b26c0728d5n%40googlegroups.com.

kavin murugam

unread,
Oct 17, 2025, 9:06:24 AMOct 17
to material...@googlegroups.com
Hi, 
What was your heat input reading?

Thank you & Stay Safe!

 

KAVIN MURUGAM

+60126159644



Saurabh Jain

unread,
Oct 17, 2025, 10:12:35 AMOct 17
to material...@googlegroups.com

Vishwas Keskar

unread,
Oct 17, 2025, 10:40:46 AMOct 17
to material...@googlegroups.com

Saurabh Jain

unread,
Oct 17, 2025, 11:05:41 AMOct 17
to material...@googlegroups.com

kavin murugam

unread,
Oct 17, 2025, 12:46:37 PMOct 17
to material...@googlegroups.com
Heat input below 2.0 Hardness achieveable, do check on your material grade & weld consumables used , i need more infro material grade & what weld process , is the any PWHT requirement? 


Thank you & Stay Safe!

 

KAVIN MURUGAM

+60126159644

Mohd Siraj

unread,
Oct 22, 2025, 12:40:52 PMOct 22
to Materials & Welding
hi  Saurabh,

would pl share who was manufactures of B.M?
now a days MTC's r not reliable..

Reply all