Weldability of A283 Gr C with A573 Gr70

100 views
Skip to first unread message

Benaouda Mezrar

unread,
Jan 25, 2023, 11:32:19 PM1/25/23
to Materials & Welding
Dear friend 

could anyone answer my question, the question is : could we weld A573 GR70 with A283GR C
In my opinion we can't  weld them because the minimum specified  tensile are 
for A283 GR C = 380 MPA
for A573 Gr70 = 485 MPA

Please friend help me i need this information emergency

if the answer is yes which type of filler metal we should use for SMAW 




 

james gerald

unread,
Jan 26, 2023, 1:40:15 AM1/26/23
to material...@googlegroups.com
Use E7018 / E7018-1


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/20e0e61e-9ee4-4ef3-9080-fe83ae9c39ban%40googlegroups.com.

Benaouda Mezrar

unread,
Jan 26, 2023, 4:12:21 AM1/26/23
to material...@googlegroups.com
But sir we use these two nuances for construction of storage tanks. Is it applicable ? with different thickness 
sir please could you give me more arguments about the weldability of these two nuances ? 
thank you a lot for your helps sir    

james gerald

unread,
Jan 26, 2023, 4:24:13 AM1/26/23
to material...@googlegroups.com

Benaouda Mezrar

unread,
Jan 26, 2023, 11:21:39 PM1/26/23
to material...@googlegroups.com

james gerald

unread,
Jan 26, 2023, 11:21:41 PM1/26/23
to material...@googlegroups.com
Also provide the thickness 

Benaouda Mezrar

unread,
Jan 27, 2023, 3:05:38 AM1/27/23
to material...@googlegroups.com
A573 gr 70 12mm 
A283 gr C 10mm

james gerald

unread,
Jan 28, 2023, 12:41:07 AM1/28/23
to material...@googlegroups.com
There are certain factors to be considered while selecting the welding consumable.

1. The Tensile strength of the welding consumable shall be higher than the minimum specified Tensile strength of the Base material.
2. If two different grades are welded the welding consumable tensile strength shall be higher than the lowest grade.
Inline image

3. If it is a structural weld and welding to the pressure boundary then low H2 electrode is preferred such as E7018 / E7108-1.

4. If it is between a non pressure part to non-pressure part then  you can prefer E6013 for your requirement and thickness.
Inline image
5. If the Thickness(>25mm) & Carbon equivalent is higher it is preferred to weld with a low H2 electrode such as E7018

Thanks & Regards

J.Gerald Jayakumar