Hi all welding experts

I have to qualify some procedures as per API 1104 and I have least knowledge about this specification.....

First I will detail my Product

1).I have Pipe( API 5L X65 MS) to be welded with a flange(ASTM A 694F65) 75deg groove angle butt joint( V groove 75 deg included angle)

2) SamePipe will be welded with a nozzle
(ASTM a694 F65) set on joint groove fillet weld.

As per API 1104 Clause 5.4.2.2 (c) for question no. 1, whether I have to make two pqr of F65 to F65 and X65 to X65 combinations with V groove 75 deg included angle??
and
as per API 1104 Clause 5.4.2.3 for question no 2 both above PQR's will suffice the requirement of nozzle to pipe welding...??


Regards

Dhanush

Lalu Rajendran

unread,
Mar 12, 2016, 4:20:18 AM3/12/16
to material...@googlegroups.com
Hi Dhanush,

As per API 1104, "A major change in joint design (e.g. from V groove to U groove) constitutes an essential variable"
You can use the same PQR (X65 to X65) with 75deg groove angle butt joint. But you must show the joint details in your wps (see below).

Inline image 1

Experts, correct me if I am wrong.

regards,
LALU



Dhanush


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/fb33ec56-f706-43b0-a5cb-77b1b3c08859%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

JIJILAL K M

unread,
Mar 12, 2016, 9:18:15 AM3/12/16
to material...@googlegroups.com
Dear Dhanush,

you need to qualify  a pqr for pipe grade X65 to X65  using a wps having E-6010 and E-7018 /16 electrode  with SMAW process since both pipe  and flanges are having similar mech. & chem. properties .
see the attachments.

his will meet all your requirements.

Dear experts ,please correct me ,If my recommendations need further fine tuning.

Regards,

JIJILAL K.M.
QA/QC Manager,Jurong Engg. ltd.
Bangkok, Thailand​



Seamless Pipes - API 5L grade X65 PSL 2.pdf
ASTM-A694-F65.pdf

Johnson Prabu

unread,
Mar 14, 2016, 9:05:19 AM3/14/16
to material...@googlegroups.com
Dear Dhanush,

1. X65 to X65 is sufficient
2. Separate qualification is required . See 5.7 and 5.8 

Regards,
Johnson Prabu



From: JIJILAL K M <jijil...@gmail.com>
To: material...@googlegroups.com
Sent: Saturday, 12 March 2016 5:16 PM
Subject: Re: [MW:24508] Procedure Qualifications as per API 1104

Reply all
Reply to author
Forward
0 new messages