Regarding brand name of welding consumable.

127 views
Skip to first unread message

Umang Parikh

unread,
Aug 30, 2017, 3:34:39 AM8/30/17
to material...@googlegroups.com
Dear friends,
Please clarify below point.( This is one of the project spec.)

"Any change in brand name of the filler metal if the service is sour"

What is the meaning of this sentence.
Is it mean to say change in the company name or company product name.
i.e ESAB TO ESAB or
its product OK TIGROD 16.30 TO OK TIGROD 16.10.

Can we make WPS of 316L with supporting PQR 304L if the above clause is essential variable as per project spec.

Appreciate to have views on above point ASAP 

Kannayeram Gnanapandithan

unread,
Aug 30, 2017, 9:32:53 AM8/30/17
to materials-welding

No

On 30-Aug-2017 1:25 pm, "Umang Parikh" <parikh...@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (parikh...@gmail.com) Add cleanup rule | More info
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

james gerald

unread,
Aug 30, 2017, 10:08:31 AM8/30/17
to material...@googlegroups.com
It is change from OK TIGROD16.30 to OK TIGROD16.10, For Sour Service as defined by the Materials Engineer with certain PPM & PH of H2S, the above change is an essential variable.


 
Thanks & Regards
J.Gerald Jayakumar
0091-9344954677



From: Umang Parikh <parikh...@gmail.com>
To: material...@googlegroups.com
Sent: Wednesday, August 30, 2017 11:34 AM
Subject: [MW:26764] Regarding brand name of welding consumable.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

PREM SHANKARDUTT NAUTIYAL

unread,
Aug 31, 2017, 8:07:57 AM8/31/17
to material...@googlegroups.com

ESAB is the welding consumable manufacturer name whereas OK TIGROD 16.30 is the Brand Name.
Hence in this case the change in brand name is an essential variable.

Regards

Prem Nautiyal


On Wed, 30 Aug 2017 19:38:26 +0530 "'james gerald' via Materials & Welding" wrote

> It is change from OK TIGROD16.30 to OK TIGROD16.10, For Sour Service as defined by the Materials Engineer with certain PPM & PH of H2S, the above change is an essential variable.

Thanks & RegardsJ.Gerald Jayakumar0091-9344954677

From: Umang Parikh
To: material...@googlegroups.com
Sent: Wednesday, August 30, 2017 11:34 AM
Subject: [MW:26764] Regarding brand name of welding consumable.

Dear friends,Please clarify below point.( This is one of the project spec.)

"Any change in brand name of the filler metal if the service is sour"
What is the meaning of this sentence.Is it mean to say change in the company name or company product name.i.e ESAB TO ESAB orits product OK TIGROD 16.30 TO OK TIGROD 16.10.

Can we make WPS of 316L with supporting PQR 304L if the above clause is essential variable as per project spec.
Appreciate to have views on above point ASAP



--

https://materials-welding.blogspot.com/

https://www.linkedin.com/groups/122787

---

You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

Visit this group at https://groups.google.com/group/materials-welding.

For more options, visit https://groups.google.com/d/optout.






--
>
https://materials-welding.blogspot.com/
>
https://www.linkedin.com/groups/122787
>
---
>
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
>
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
>
Visit this group at https://groups.google.com/group/materials-welding.
>
For more options, visit https://groups.google.com/d/optout.
>


PREM S NAUTIYAL
CELL : 9769316004

Neilashkumar

unread,
Aug 31, 2017, 12:33:06 PM8/31/17
to material...@googlegroups.com
Hi all, 

Normally for sour service application , brand is an essential variable only for Nickel base and duplex consumable  . Trade name may vary and can be changed as long as same F number and A number is matching need to make one additional supplement chemical analysis and you may proceed  if client agrees.
This is my suggestion only.

P.NEILASHKUMAR 
Sent from my iPad
MOB : 966 551094590