Impact test for PQR

158 views
Skip to first unread message

Chintan

unread,
Mar 3, 2020, 12:07:09 AM3/3/20
to Materials & Welding
Kindly advice how many set of impact test (for each process)needs to run to qualify PQR with below details
What is code ref for pqr impact test

Base metal thick 50 mm
Process GTAW (5mm) + FCAW (20 mm) + SAW (25 mm)
Governing code asme sec 8 div 1 & asme sec 9
MDMT minus 29 deg cel

Ramesh

unread,
Mar 3, 2020, 3:32:37 AM3/3/20
to material...@googlegroups.com
Pl check UG-84 & UCS 67  in ASME Sec 8 Div.1. 

Thanks and Regards


Rameshkannan Devaraj

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/be15deb6-c237-4b43-9194-cdb198cb41a0%40googlegroups.com.

Fernando L Neto

unread,
Mar 4, 2020, 3:30:31 AM3/4/20
to material...@googlegroups.com
Hello, colleagues. 

This is also my doubt. 

UG-84 does not require impact sets for each process. quantity of sets is defined only based on base metal thickness. Am I correct? 

Are additional impact sets for each process supplementary requirement in addition to ASME requirements? 

Best regards, 

Fernando L Neto

unread,
Mar 4, 2020, 3:30:31 AM3/4/20
to material...@googlegroups.com
Sorry.

Regarding the last edition of ASME VIII, there is specific mention to multiple processes. 

Best regards

Kannayeram Gnanapandithan

unread,
Mar 4, 2020, 4:35:53 AM3/4/20
to materials-welding
Pl ref QW 200-4, a(1).   and  UG-84- Charphy Impact Test, (h), (5). It is clearly given for multiple welding process. 

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


Pipeline Welding

unread,
Mar 5, 2020, 1:39:23 AM3/5/20
to Materials & Welding
Weld Metal = 2 Location
HAZ = 2 Location

Ref:
Applicble Code = ASTM A 370 & ASME B31.3
ASME BPVC.IX - Figure QW-463.1(f) Toughness Test Specimen Location

james gerald

unread,
Mar 5, 2020, 2:59:30 AM3/5/20
to material...@googlegroups.com
Dear,

Requirement for each welding process to Impact testing is not a Sec.8 or Sec.9 requirement of ASME Code but this will be a requirement in some Client specifications.

Please see Sec.8 requirements below snap shot.

Inline image
Inline image


Thanks & Regards

J.Gerald Jayakumar

0091-6382552037



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit

Kannayeram Gnanapandithan

unread,
Mar 6, 2020, 12:14:31 AM3/6/20
to materials-welding
Ref the below attachment taken from ASME sec 8, Div1, UG 84, h, 5.  Hope that it will clear your doubts. 

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Tue, Mar 3, 2020 at 10:37 AM Chintan <chin...@gmail.com> wrote:
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
UG 84, h, 5.docx

james gerald

unread,
Mar 7, 2020, 4:50:02 AM3/7/20
to material...@googlegroups.com
What is the version(year)  of code.

Thanks & Regards

J.Gerald Jayakumar


james gerald

unread,
Mar 7, 2020, 4:50:02 AM3/7/20
to material...@googlegroups.com
Pandithan Sir,  Thanks for your reference and it belongs to ASME 2019 Code.

This is a Learning Forum where everybody gets benefitted from the Inputs from all Individuals.

Appreciate your Time for all Inputs

Thanks & Regards

J.Gerald Jayakumar


On Friday, March 6, 2020, 12:15:24 PM GMT+7, Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote: