PWHT time calculation

3,306 views
Skip to first unread message

Student

unread,
Oct 7, 2022, 1:43:15 AM10/7/22
to Materials & Welding
Dear All
Please guide how to calculate the rate of heating for PWHT for below AWS d1.1

"Para 7.8.1 Above 600°F [3 1 5 °C] , the rate of heating in °F [°C] per hour shall not exceed 400 [560] divided by the maximum
metal thickness of the thicker part, in inches [centimeters ] , but in no case more than 400°F [220°C] per hour"

If the maximum thickness is 2 inches , how to calculate heating rate

Rathinavel Arumugam

unread,
Oct 7, 2022, 2:32:47 AM10/7/22
to material...@googlegroups.com
As per 7.8.1, para 2,
rate of heating ia 560/2"= 280Deg.C

But there is a condition that "but in no case more than 220Deg.C per hour.

Hence you have to apply 220 Deg. C per hour. 



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/007241e8-ef96-424b-b22f-136b00673b26n%40googlegroups.com.

manohar g

unread,
Oct 7, 2022, 5:13:21 AM10/7/22
to material...@googlegroups.com

Dear Nabeel,

As per AWS D1.1, rate of heating shall not exceed 400°F (560°C) divided by max. Metal thickness of thicker part, in inches (cm), but in no case more than 400°F (220°C) per hour.

If the maximum thickness is 2” (5.08cm), rate of heating will be

400°F / 2” = 200°F per hour.

Or

560°C / 5.08cm = 110°C per hour

Hence, for 2 inch thick, rate of heating shall not exceed 200°F per hour or 110°C per hour.

Note : If the calculated rate of heating temperature is more than 220°C, consider rate of heating max. 220°C.

 

As per ASME Sec. VIII Div. 1, rate of heating shall be not more than 400°F/hr (222°C/h) divided by the maximum metal thickness of the shell or head material in inches, but in no case more than 400°F/hr (222°C/h).

 

If the maximum thickness is 2”, rate of heating will be

400°F / 2” = 200°F per hour.

Or

222°C / 2” = 111°C per hour.


Regards,


G.Manohar