E7018 & E7018-1

6,972 views
Skip to first unread message

Adi

unread,
Nov 6, 2010, 10:15:41 AM11/6/10
to Materials & Welding
Hi everybody

What is meaning of " -1 " in electrode E7018-1
Is it indicate hydrogen diffusion

What is the difference between E7018 & E7018-1, only impact test or
material composition also


Reg

aneesh

unread,
Nov 7, 2010, 1:07:32 AM11/7/10
to material...@googlegroups.com
Hai,

"-1"  designate that the electrode meets the requirement of improved toughness or impact.

"HZ" is using to designate the hydrogen diffusion. ie 'Z' ml of Hydrogen per 100g of deposited metal, where Z=4,8 or 16 (refer ASME Sec II part C SFA 5.1 or AWS A5.1)

E7018-1 have same usability and weld metal composition as E7018, except the manganese content set high range  and these electrodes are intended for welds requiring a lower transition temperature than is normally available from E7018 electrodes.

E7018  avg min impact 27J @ -30DegC

E7018-1 avg min impact 27J @ -45DegC


Regards,
Aneesh
KSA

On Sun, 07 Nov 2010 08:13:27 , Adi wrote
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

george....@gr.bureauveritas.com

unread,
Nov 7, 2010, 8:48:55 AM11/7/10
to materials-welding
Improved impact properties

Chandulal Vithlani

unread,
Nov 8, 2010, 12:46:56 AM11/8/10
to material...@googlegroups.com

Can any throw light why water filling is needed for such a functional test?

 

Chandulal S Vithlani

050 614 2950

 

**********************************************************************

Borouge is a leading provider of value creating, innovative plastics solutions for customers in the Middle East, Asia-Pacific and Africa. Borouge employs unique Borstar® technology to produce differentiated products for high-value infrastructure applications, including water, gas and industrial pipe systems, power and communication cables, advanced packaging and automotive components. Borouge’s state-of-the-art petrochemical complex is located at Ruwais, Abu Dhabi in the United Arab Emirates.

===================================================================================
CONFIDENTIALITY NOTICE

This email and any files transmitted with it are confidential and intended solely for the use of the individual or entity to whom they are addressed. If you have received this email in error please delete the email and any attachment(s) and notify the sender.

This footnote also confirms that this email message has been scanned for the presence of computer viruses.
=============================================================================================================

 

M.Shankar

unread,
Nov 8, 2010, 8:07:25 AM11/8/10
to material...@googlegroups.com
What is meaning of " -1 " in electrode E7018-1

The (-1) = low temp impact
Refer ASME Sec II Part C –Specifications for Welding Rods, Electrodes,and FillerSFA 5.1:
A “−1” designator following classification identifies an electrode which meets optional supplemental impact requirements at a lower temperature than required for the classification


Is it indicate hydrogen diffusion

No. but in E7018-1H4R
H4 = hydrogen diffusion level 4 mL(H2)/100g.
R   = meets moisture test



What is the difference between E7018 & E7018-1, only impact test or

material composition also

Refer ASME Sec II Part C –Specifications for Welding Rods, Electrodes,and Filler - SFA 5.1:
E7018-1 having an increase in the manganese content could reduce the Ductile/Brittle " transition" temperature and improve the low temperature impact values of the weld metal.



From: "george....@gr.bureauveritas.com" <george....@gr.bureauveritas.com>
To: materials-welding <material...@googlegroups.com>
Sent: Sun, 7 November, 2010 9:48:55 PM
Subject: Re: [MW:8120] E7018 & E7018-1

Improved impact properties


----- Original Message -----
From: Adi [adin...@gmail.com]
Sent: 06/11/2010 07:15 MST
To: "Materials & Welding" <material...@googlegroups.com>
Subject: [MW:8112] E7018 & E7018-1



Hi everybody

What is meaning of " -1 " in electrode E7018-1
Is it indicate hydrogen diffusion

What is the difference between E7018 & E7018-1, only impact test or
material composition also


Reg

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

tedr...@gmail.com

unread,
Oct 21, 2016, 4:18:27 AM10/21/16
to Materials & Welding, chandulal...@borouge.com
Hi Chandulal

This test is related to anodic and cathodic protection of metal structures. Two different metals can stand near each other in air without having any effect on each other, as air space is an insulator). When the metals are in water (an electrolyte) it's a different story as they are able to form an electrical bond through the water (water is generally regarded as a conductor). Differing metals occupy a different position on the Anodic Index, with some being described as more noble than others. The more noble metal is less susceptible to galvanic corrosion than the less noble. To protect the less noble steel from attack, a sacrificial anode is attached to it, which will be eaten away instead of metal. This whole process only takes place in an electrolyte, in this case, water. It's a problem in the marine world, but without this process we generally wouldn't have batteries in the form we know them, and the very protective coating known as galvanising originates here too.

Cheers

John