Dear All,
 
I want to prepare a WPS for ,
 
material ASTM B 423 (P No-45).
 
Process - GTAW
Construction Code - ASME B31.3
Welding Code - ASME BPV SEC IX
 
What is the F - No. of ERNiCrMo-3?  43 or 45?One of the  WPS in my hand says 45 !!!
I have reviewed ASME BPV SEC IX QW 432,F-No. section and found that 43.Now I need clarification from experts,which one is correct 43 or 45?
 
What is the A - No. of ERNiCrMo-3? I have reviewed QW 422 A-Numbers section,but couldn't find.
 
Is there any condition that P- no. and F- no. shall be same?
 
Seniors, I need your help on this issue.
 
 
Regards,
 
Limesh

Raghuram Bathula

unread,
Sep 18, 2010, 12:23:43 PM9/18/10
to material...@googlegroups.com
For ERNiCrMo-3 Fnumber is 43, please recheck WPS if they have specified some other filler such as NiFeCr-1, NiCrMo-9 falls under F45.
A Numbers are not applicable for non ferrous welds

No such condition as for P number/F Number should be same in Sec IX.

César Alexis Viteri Pérez

unread,
Sep 18, 2010, 2:55:13 PM9/18/10
to material...@googlegroups.com
 

Dear All,

I’m going to make some Works inside of a dehydrator (please see attachment), the questions are:

  1. If I cut the angle suports without Couch the shell, do i need an R stamp company for mantain the ASME stamp?
  2. If I cut the angle suports and grinding the angle flush to shell, do i need an R company for mantain the ASME stamp?
  3. For cutting the existents excentric reducers as and Weld others, do i need an R company for mantain the ASME stamp?

 

Please escuse my language, i’m not native speaker (or writer :D )

Thank in advance for your cooperation.

 


 

Date: Sat, 18 Sep 2010 21:53:43 +0530
Subject: Re: [MW:7079] F-No&A-No of ERNiCrMo-3
From: raghura...@gmail.com
To: material...@googlegroups.com
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
VESSEL ANGLE.jpg

Karthik

unread,
Sep 20, 2010, 3:26:12 AM9/20/10
to material...@googlegroups.com

Hi,

P.Number and F number are different and the numbers cannot be same and substituted.

For ERNiCrMo-3 F-Number is 43. For A number You can check with the QW-442 along with your Filler metal certificate to compare the chemical composition.Since it is a nickel based alloy,you check with the composition of A number 10 requirments.

 

Pls.find below the extraction of ASME appropriate sections. 

 

QW-404.37

A change in the composition of the deposited

weld metal from one A-Number in table QW-442 to

65

any other A-Number, or to an analysis not listed in the table.

Each AWS classification of A-No. 8 or A-No. 9 analysis of

table QW-442, or each nonferrous alloy in table QW-432,

shall require separate WPS qualification. A-Numbers

QW-404.5

(Applicable only to ferrous metals.) A

change in the chemical composition of the weld deposit

from one A-Number to any other A-Number in table

QW-442. Qualification with A-No. 1 shall qualify for

A-No. 2 and vice versa.

The weld metal chemical composition may be determined

by any of the following:

(a)

For all welding processes—from the chemical analysis

of the weld deposit taken from the procedure qualification

test coupon.

(b)

For SMAW, GTAW, and PAW — from the chemical

analysis of the weld deposit prepared according to the

filler metal specification, or from the chemical composition

as reported either in the filler metal specification or the

manufacturer’s or supplier’s certificate of compliance.


Thanks & Regards,
 
(Karthik)
Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Sat, 9/18/10, limesh M <lime...@gmail.com> wrote:

sunil mani

unread,
Sep 20, 2010, 4:15:05 AM9/20/10
to material...@googlegroups.com
Dear Raghuram sir,
 
I have reviewed my WPS and the following values observed.
 

Specification (SFA)  :  A 5.14(GTAW)

AWS classification   :  ER-NiCrMo-3(GTAW)

Trade Name            :  Thermanit625(GTAW)
 
 Filler metal product form : Solid (GTAW) 
 
Chemical composition in % for GTAW: C-0.008%, Si-0.06%, Mn-0.02%,Cr-22.32%,
Mo-8.93%, Nb-3.53%, Ni-64.10%,Fe-0.439%,P-0.001%,S-0.001%,Cu-0.039%,Ti-0.181% &Al-0.127%
 
 
Dear Karthik Sir,
 
Thank you for the correction,I had mistakenly typed QW.422 instead of QW.442
 
I have reviewed ASME QW.422 'A' No. section and couldn't find any matching chemistry with above mentioned chemical composition.
 
In this case,In the A-No column of WPS, what I have to write? N/A or Nil?
 
 
 
Regards,
 
 
Limesh

Bathula Raghuram (Mumbai - PIPING)

unread,
Sep 20, 2010, 4:29:34 AM9/20/10
to material...@googlegroups.com

F number will be 43 and A number is not applicable for non ferrous materials

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of sunil mani
Sent: Monday, September 20, 2010 1:45 PM
To: material...@googlegroups.com
Subject: Re: [MW:7103] F-No&A-No of ERNiCrMo-3

 

Dear Raghuram sir,

 

I have reviewed my WPS and the following values observed.

 

Specification (SFA)  :  A 5.14(GTAW)

AWS classification   :  ER-NiCrMo-3(GTAW)

Trade Name            :  Thermanit625(GTAW)

 

 Filler metal product form : Solid (GTAW) 

 

Chemical composition in % for GTAW: C-0.008%, Si-0.06%, Mn-0.02%,Cr-22.32%,

Mo-8.93%, Nb-3.53%, Ni-64.10%,Fe-0.439%,P-0.001%,S-0.001%,Cu-0.039%,Ti-0.181% &Al-0.127%

 

 

Dear Karthik Sir,

 

Thank you for the correction,I had mistakenly typed QW.422 instead of QW.442

 

I have reviewed ASME QW.422 'A' No. section and couldn't find any matching chemistry with above mentioned chemical composition.

 

In this case,In the A-No column of WPS, what I have to write? N/A or Nil?

 

 

 

Regards,

 

 

Limesh

 On Mon, Sep 20, 2010 at 11:26 AM, Karthik <karth...@yahoo.com> wrote:

Hi,

P.Number and F number are different and the numbers cannot be same and substituted.

For ERNiCrMo-3 F-Number is 43. For A number You can check with the QW-442 along with your Filler metal certificate to compare the chemical composition.Since it is a nickel based alloy,you check with the composition of A number 10 requirments.

 

Pls.find below the extraction of ASME appropriate sections. 

 