Dear All,
 
Can Any one Explain me what is the difference between API 5L PSL-1 and PSL-2.What is the signefecance and where we need to use the specific PSL.
 
Regards,
 
Prakash K B

rake...@rediffmail.com

unread,
Jan 4, 2010, 11:30:39 AM1/4/10
to material...@googlegroups.com
Dear Prakash
The differences are given in API 5L in the end pages.
The application depends on the project spec, client spec etc. Product Specification Level(psl) 2 is stringent.
Rakesh Pandey

Empower your Business with BlackBerry® and Mobile Solutions from Etisalat


From: prakash kamathuru <praka...@gmail.com>
Date: Mon, 4 Jan 2010 22:21:40 +0800
Subject: [MW:3957] API 5L -PSL 1 & PSL 2
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Chandra Bhusan Tripathi

unread,
Jan 4, 2010, 8:02:56 PM1/4/10
to praka...@gmail.com, material...@googlegroups.com
Please refer to API table in appendix, It is the level of inspection on PSL2 pipes that make it diferent from PSL1. PSL2 is mostly used in pipeline where visula inspection of pipen after construction/during hydrotest is of great concern. PSL 1 are used either for structure or can be used for plant piping where visual inspection during construction is not a concern. API doesnot make mendatory to have MTC for PSL1 pipe, since most of the API pipes are dual cartified you can ask for MTC from trader/manufacturer.

Regards

Chandra
On Mon, 04 Jan 2010 21:31:23 +0530 wrote

>Dear All,
 
Can Any one Explain me what is the difference between API 5L PSL-1 and PSL-2.What is the signefecance and where we need to use the specific PSL.
 
Regards,
 
Prakash K B



--
>
To post to this group, send email to material...@googlegroups.com
>
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>


Chandra Bhusan Tripathi
23 Beckett Circle
Perth, WA
Australia
M +61422812970
H +61862012197

Ramprasad Chari

unread,
Jan 4, 2010, 11:45:41 PM1/4/10
to material...@googlegroups.com
PSL is "Product Specification Level".In case of PSL-1 impact testing is not mandatory and in case of PSL2 impact testing at 0 deg C is mandatory.There is a difference in Chemical composition requirements between PSL1 and PSL2.In case of PSL1 Yield Stress and UTS demands "min" value whereas in case of PSL2 there is a range of "min" and "max" for YS and UTS.
Regards

--

kayvan alyari

unread,
Jan 17, 2010, 2:23:29 AM1/17/10
to material...@googlegroups.com
--
PSL 1 & 2.pdf

Paul Jevons

unread,
Jan 17, 2010, 7:44:33 PM1/17/10
to material...@googlegroups.com
PSL-2 has more stringent testing requirments. Refer to API 5L which details the differences. It is common practice to go with PSL-2 requirments as default unless requested by the client.
 
PJ

sachin sankhe

unread,
Jan 17, 2010, 9:19:26 AM1/17/10
to k.al...@gmail.com, material...@googlegroups.com

Hi,

There is lot of differnces b/w PSL1 & PSL2
PSL 2 has got more stringent requirement than PSL 1 like impact requirement,etc
For detail difference refer Appendix J of API 5L

Regards
Sachin.Sankhe

On Sun, 17 Jan 2010 19:29:26 +0530 wrote

>
On 1/4/10, prakash kamathuru wrote:

Dear All,
 
Can Any one Explain me what is the difference between API 5L PSL-1 and PSL-2.What is the signefecance and where we need to use the specific PSL.
 
Regards,
 
Prakash K B
-- To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

ashraf aly

unread,
May 19, 2013, 7:11:07 AM5/19/13
to material...@googlegroups.com
Dear Parakash

as mentioned in API 5L the main difference between PSL2 and PSL 1 that PSL2 can
resist low temperature services , so impact test is mandatory for PSL2, also you find
some chemical analysis  changes and related mechanical properties between PSL1 and PSL2

 
Best regards

Ashraf Aly
Bureau Veritas Egypt


From: Bruno Luchessi <brunol...@gmail.com>
To: material...@googlegroups.com
Sent: Saturday, May 18, 2013 8:25 PM
Subject: [MW:17699] Re: API 5L -PSL 1 & PSL 2


In the preparation of this second edition of ISO 3183, the technical committee recognized that there are two
basic levels of standard technical requirements for line pipe and, therefore, agreed to establish requirements
for two product specification levels (PSL 1 and PSL 2). Level PSL 1 provides a standard quality level for line
pipe. Level PSL 2 has additional mandatory requirements for chemical composition, notch toughness and
strength properties and additional NDE. Requirements that apply to only PSL 1 or to only PSL 2 are so 
designated. Requirements that are not designated to a specific PSL designation apply to both PSL 1 and
PSL 2. A table comparing this edition of ISO 3183 with the with the predecessor International Standard
ISO 3183 (all parts) and API Spec 5L and used in the harmonization of these documents is given for
information in Annex M. 
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/

 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


Narayanan, Jyothidas [Heston]

unread,
May 19, 2013, 8:14:56 AM5/19/13
to material...@googlegroups.com

API 5L GR. B PIPES

PROPERTIES / REQUIREMENTS COMPARISON SHEET FOR PSL 1 & PSL 2 PIPES

Sl. No.

Properties

REQUIREMENTS

ACTUAL SEAMLESS PIPES USED (Heat Nos.)

API 5L Gr. B PSL 1

API 5L Gr. B PSL 2

1

2

3

4

5

6

 

 

 

 

68B2583 (4")

88B8482 (4")

89B0779 (6")

89B5553 (6")

0000213182 (6")

0000213415 (6")

 

Chemical Composition

 

 

 

 

 

 

1

C % max.

0.28

0.24

0.16

0.18

0.16

0.168

0.15

0.15

2

P % max.

0.03

0.025

0.018

0.006

0.006

0.013

0.01

0.01

3

S % max.

0.03

0.015

0.002

0.004

0.003

0.003

0.003

0.003

4

Mn % max.

1.20

1.20

0.80

0.85

0.81

0.82

0.74

0.74

5

Si % max.

NS

0.40

0.26

0.29

0.24

0.24

0.26

0.26

6

CE (Carbon Equivalent) % max.

NS

0.43

0.33

0.348

0.34

0.347

0.32

0.32

 

 

 

 

 

 

 

 

 

 

 

Mechanical Properties

 

 

 

 

 

 

7

Yield Strength MPa (min. / max.)

245 / NS

245 / 450

342, 345

347, 344

336, 334

331, 333

301, 293

305, 294

8

Tensile Strength MPa (min./ max.)

415 / NS

415 / 760

527, 534

493, 489

519, 507

497, 497

477, 467

482, 469

9

Fracture Toughness (CVN Impact Test)

NS

Table 8/18/22 (NA)

NA

NA

NA

NA

149, 147 (J)

149, 187 (J)

 

 

 

 

 

 

 

 

 

 

 

Non-Destructive Inspection

 

 

 

 

 

 

10

EM / UT / MPI

Any method

Any method

EM

EM

EM

EM

EM

EM

 

 

 

 

 

 

 

 

 

 

 

Other Tests

 

 

 

 

 

 

11

Hydrotest

Each Pipe

Each Pipe

done

done

done

done

done

done

12

Hardness Test (max.)

Table 17 (NA)

Table 18 (NA)

163, 165 (HV 30)

151, 152 (HV 10)

149, 152 (HV 30)

148, 149 (HV 10)

76, 75 (HRB)

76, 75 (HRB)

13

NACE Compliance

NS

NS

written in MTC

written in MTC

written in MTC

written in MTC

written in MTC

written in MTC

 

 

 

 

 

 

 

 

 

 

 

Note: NS - Not Specified; NA - Not Applicable. Only 6 Heats of Seamless Pipes are listed here.

 

 

 

 

 

 

 

 