Your reasoning is flawed and your answer incorrect.
Another example of reading the QW-4xx variables out of context.
QW-405.2 typically applies to general process qualification (groove welds, etc.).
QW-405.4 apples to special process qualifications (Hard facing or corrosion resistant overlay).
These two variables are never called out together.
Regarding the application of supplementary essential variable QW-405.2, I suggest you read Interpretation IX-81-24 reply to question 1 states :
Reply (1): When applying QW-405.2, any position not involving the vertical uphill progression will qualify for all positions, except those involving the vertical uphill progression. Any position involving the vertical uphill progression win qualify for all positions, including those involving the vertical uphill progression. For example, qualification on a test coupon in the 2G position will qualify 4G and 5G downhill, but not 3G uphill. Qualification on a test coupon in 3G uphill progression will qualify 4G, 6G uphill progression, and all other positions.
John A. Henning
Welding & Materials
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
You may use E 8018 B2
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/77079F5DE5B54356AFDB6EB0C5C49519%40mechworkshop.
ER80S- B2 + E8018 B2
Hi, i want to ask what is the difference between uphill and downhill in ASME IX and API 1104? The second question is why the ASME IX qualified uphill and downhill as uphill not qualified API 1104 downhill.
Hi, i want to ask what is the difference between uphill and downhill in ASME IX and API 1104? The second question is why the ASME IX qualified uphill and downhill as uphill not qualified API 1104 downhill.Thank you and hope get answer...hehehehee
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/5374f869-a190-498a-bda1-f4531d39f161%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
When impact is there, 3G Uphill qualify all positions
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40DPzq%3Dx_0LjxyW9X%3D_s80FySNyRxhZ5uk%3DCJHgkz0KQHw%40mail.gmail.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNiUTqGEPPtQdiaojtGC0WzM8V9iAuZjdzdVAoD%3DONBrg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
Dear Sir,
It states of PQR is qualified with 1G position then it will qualify for all positions, if there is no impact requirements in job and wps can be used for all positions for non impact requirement.
And if PQR is qualified for 1G position and if we will have to support it with impact requirement job , then WPS will be used for 1G position only.
With impact PQR should be qualified in either 3G in case of plate and In 5G or 6G in case of pipe to qualify all positions with impact requirement.
Regards,
Mohit Aggarwal.
Sr. Engineer-Welding.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALTezPNee2_tWR54mdxNEXuuc0UCAAStyvRXd6wuL5LC2%3D10Jg%40mail.gmail.com.