please guide me exactly how many percentage and which area i should select for RT for API 650 tank for below joints.

1) shell verticle
2) shell horizontal
3) shell intersections (verticle to horizontal)
4) nozzles

i checked API 650 but not getting clear picture hence request to provide standard practice in this regard.

regards,
sam.

Thota Kishore

unread,
Nov 6, 2013, 3:31:41 PM11/6/13
to material...@googlegroups.com
Dear Sam

Refer Para 8.1.2.2 and 8.1.2.3 in API 650.

It clearly states about the location and number of radiographs in tank.


Thanks & Regards,

T KISHORE
Engineer-QA/QC
+91 9951141681

*P** **I Pledge to take personal action to help solve the climate
crisis by reducing my own CO2 pollution as much as I can offsetting the
rest to become "Carbon Neutral". *
*
*
*Spread environmental awareness to avoid Global Warming. *
* *
*Save Nature... Save Future...*

**

Perumal Govindan

unread,
Nov 6, 2013, 7:26:33 AM11/6/13
to material...@googlegroups.com
Mr Sam,

Further refer also API 650 Section 8.1.1, 8.1.2.2, 8.1.2.9.

P Govindan


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

Perumal Govindan

unread,
Nov 6, 2013, 7:22:22 AM11/6/13
to material...@googlegroups.com
Mr Sam 

Refer API 650 Appendix T NDE requirements summary.

Regards
P Govindan


On Wed, Nov 6, 2013 at 12:24 PM, Sam <onlypri...@gmail.com> wrote:

S DAS Arun RSHT-2

unread,
Nov 7, 2013, 1:56:53 AM11/7/13
to material...@googlegroups.com

Dear Sam,

Please find below the extract from API 650.

 

 

 

Hope this will help is interpreting the requirements.

 

Regards,

 

Arun

 

 


 
Nota di riservatezza : Il presente messaggio, corredato dei relativi allegati, contiene informazioni da considerarsi strettamente riservate, ed è destinato esclusivamente al destinatario sopra indicato, il quale è l'unico autorizzato ad usarlo, copiarlo e, sotto la propria responsabilità, diffonderlo. Chiunque ricevesse questo messaggio per errore o comunque lo leggesse senza esserne legittimato è avvertito che trattenerlo, copiarlo, divulgarlo, distribuirlo a persone diverse dal destinatario è severamente proibito, ed è pregato di rinviarlo immediatamente al mittente distruggendone l'originale.
Grazie

Confidentiality Notice : This message, together with its attachments, contains strictly confidential information and is intended only for the addressee identified above, who is the sole party authorized to use and copy it and, assuming any related liability , to forward it to others. Anyone receiving this message by mistake or reading it without authorization is hereby notified that storage, reproduction, disclosure or distribution of the message to persons other than the addressee is strictly forbidden. They are asked to return the message immediately to the sender and to erase the original message received.
Thank you

 

--

Sam

unread,
Nov 7, 2013, 12:31:44 AM11/7/13
to material...@googlegroups.com
thanks to all.
just little doubt. 

our bottom shell course requirement is 10mm as per drawing but plate shows more than 10mm actually say 10.5 mm. then do we need to apply RT criteria for more than 10 mm or not ?

Mervin

unread,
Nov 6, 2013, 9:52:26 PM11/6/13
to material...@googlegroups.com
Dear mr sam

You can refer the api-650 clause 8.1.2.2 a&b and 8.1.2.3 as mention on this paragraph only spot RT for vertical & horizontal in the 1st 3mter and we use the standard in aramco for intersection joints on top angle to shell.

Vin



Sent from my iPhone

Perumal Govindan

unread,
Nov 7, 2013, 12:57:52 PM11/7/13
to material...@googlegroups.com
Mr. Sam,
Review the MTC of plate material and tolerance of specific heat / lot number and then identify the thickness of the lowest shell course thickness.

For lowest shell course, one spot radiography on every vertical joint.

Hope this will clarifies your doubt.

P Govindan   

Devang Majithia

unread,
Nov 8, 2013, 6:19:23 AM11/8/13
to material...@googlegroups.com

 

Extract taken from API 650. Refer Figure 8.1

 

Regards

Devang Majithia


 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

Legal Disclaimer :  http://mail.gnfc.in/disclaimer
image001.png

Abd Ur Rehman

unread,
Aug 20, 2024, 2:10:38 AM8/20/24
to Materials & Welding
Dear expert 

please guide , what it means to  25 % of which shall be at intersections.

Best Regards,
Abd Ur Rehman
QA/QC Engineer

raj kumar

unread,
Aug 20, 2024, 5:53:41 AM8/20/24
to material...@googlegroups.com
In my view, 25%of total intersection/tee joints . 

However if we take 100% RT in Tee joints.No need consider intersection.


---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Reply all
Reply to author
Forward
0 new messages