Reg Flange Serration Damage

144 views
Skip to first unread message

srinivasa rao

unread,
Aug 3, 2022, 5:34:02 AM8/3/22
to material...@googlegroups.com
Dear All,

We have found Damage on the Flange Serration A 350 LF2 CL1 standard , 300 #. 
Can we make the repair by weld buildup and Make new Serration . Also is it necessary to make any Heat Treatment after the serration ?

Pls advise.

Attached photo for reference. 

Srinivas
Flange Serration Damage.jpeg

Sudhakar Kuppuswamy

unread,
Aug 3, 2022, 5:48:54 AM8/3/22
to material...@googlegroups.com
Please share the size, thickness and intended service details.   

Regards,

Sudhakar K CEng MWeldI,IWE.

Welding & Metallurgical Engineer,

Email: sudhak...@gmail.com.



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKqa_5vs9nM%3Dsaw6B_7%3DVvmGxRzj_h1wmr10fZkuNRqrkJnxaA%40mail.gmail.com.

Sudhir Kumar

unread,
Aug 3, 2022, 5:59:42 AM8/3/22
to material...@googlegroups.com
Flange serration in place is possible  without any welding (do not require PWHT). Need to hire contractor who is having specialised machine. 
As its not commonly used, service cost would me higher.

Regards 

--

Shahil Saini

unread,
Aug 3, 2022, 6:34:38 AM8/3/22
to material...@googlegroups.com
Hello sir 
Without material build up at that damage place, how machining is possible??? It will reduce the dimensions I think

Prashant Rane

unread,
Aug 3, 2022, 6:34:43 AM8/3/22
to material...@googlegroups.com
Flange serration repair is possible without weld repair if the final serrated face is 0.8 mm thick.

If welding need to be carried out it shall be as per ASME PCC2, 305, and PCC1 4, Appendix C and D

PWHT required if it is a service requirement.

Regards,
 
Prashant P Rane



Sudhir Kumar

unread,
Aug 3, 2022, 6:48:34 AM8/3/22
to material...@googlegroups.com
Serration inplace will not reduce the thickness, hardly in microns which is negligible.

Sudhir Kumar

unread,
Aug 3, 2022, 6:48:34 AM8/3/22
to material...@googlegroups.com
Not required to attend damage 100%. Serration in place shall be done for the maximum possible extent and as long as holding pressure and no leakage, no issues.

Welding is not recommended for such a minor damage.

On Wed, 3 Aug 2022, 13:34 Shahil Saini, <sainis...@gmail.com> wrote:

james gerald

unread,
Aug 3, 2022, 6:48:34 AM8/3/22
to material...@googlegroups.com, Prashant Rane
If it is a new flange rather than in service refer ASME SA350 & S50 OF SA961 for sections on repair


ALLIANCE PIPES AND FITTINGS

unread,
Aug 4, 2022, 1:35:36 AM8/4/22
to Materials & Welding
It is better to make new serration by machining, avoid any weld repair.

Regards,

Mukesh Shah
Alliance Pipes & Fittings
sa...@alliancefittings.net