Advise for Weld defects during SAW Welding

95 views
Skip to first unread message

SMM

unread,
Apr 25, 2023, 7:40:09 AM4/25/23
to Materials & Welding
Dear Experts, 

There are few issues found during SAW weld  cladding at site and are highlighted in the report. Please find attached report.

I have a few questions
1. Reason for such issue to occur. 
2. Is the issue of Flux (neutral basic flux) or Flux cored wire used in the process.
3. Please advise how can this be sorted out.

Thank you,
George
REPORT2.doc

P Goswami

unread,
Apr 25, 2023, 8:00:50 AM4/25/23
to material...@googlegroups.com

What’s the wire & flux make  being used. Do not provide the AWS grade alone , specify the make also. That’s important.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Consultant: SNC Lavalin Inc. (Nuclear &Non-Nuclear)

Saudi Aramco Approved Designated Project Welding Engineer (DPWR)

Qatar Petroleum Approved, SME-Materials & Corrosion Engineering.

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c92d0a0d-f589-47eb-8def-01c5e040a3b2n%40googlegroups.com.


Virus-free.www.avg.com

Mehrab Chakoshkar

unread,
Apr 25, 2023, 11:04:50 PM4/25/23
to Materials & Welding
Hi
First, you should give us sufficient information such as the AWS Classification, the wire and flux name, and the ASTM name of the material.
second, seemingly your welding speed has been high, I can see the long beads in the welding direction.
third, sticking the slag usually happens when the A is too high and the cause of porosity usually is moisture in the flux, have you baked the flux before use?
Mehrab

RANEESH PK

unread,
Apr 26, 2023, 1:07:39 AM4/26/23
to material...@googlegroups.com
because of very  high traveling speed and long weld bead. 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

SMM

unread,
Apr 26, 2023, 4:12:20 AM4/26/23
to Materials & Welding
Dear experts thank you for your valuable advises. 

The used consumables are
Wire : Cordiff 357 SA (Cr, Ni, Mo alloyed Tubular wire) Make - Diffusion
Flux: Supershield SS Flux ( Basic Flux, Neutral behaviour in terms of C, Cr, Ni & Mo pick-up or burn out)  Make: Super Alloys & Metals

Regards,

SMM

unread,
Apr 26, 2023, 4:12:46 AM4/26/23
to Materials & Welding
Thank you for the replies experts.

Wire used: CORDIFF 357 SA (Cr, Ni, and Mo alloyed tubular wire) Make - Diffusion
Flux used: SUPERSHIELD SS Flux Make - Super Alloys and metals (data sheet attached)

Regards,
On Wednesday, 26 April 2023 at 10:37:39 UTC+5:30 RANEESH PK wrote:
Supershield SS _ All SS_ Rev 7 Oct 13.pdf
Reply all
Reply to author
Forward
0 new messages