ASME BPV Sec VIII div1 , UCS-68(b) - PWHT requirements

Visto 161 veces
Saltar al primer mensaje no leído

Raghuram Bathula

no leída,
18 sept 2020, 23:31:2118/9/20
a Materials-Welding
Can you please provide your interpretation for the following requirements of UCS-68(b)
Vessel MDMT - 48 °C , PWHT - not required

In accordance with para UCS-68(b) PWHT is required except for Category A and B joints with 100% RT, lightly loaded attachments and seal welds only.
and it is silent on category C , D welds and other attachments.

Question: does this mean PWHT is required for Category C and D, even though it is exempted for Category A and B welds? then vessel will undergo local PWHT
In my opinion we should not interpret this way and look for only what is code specifies (i.e. if Category A and B or other welds as specified is exempted entire vessel is exempted)  

MW

no leída,
23 sept 2020, 1:36:4623/9/20
a Materials & Welding
If a weld joint has a coincident ratio higher then 0,35 then the same need to be PWHT with the following exemptions from PWHT (even if coincident ratio is higher than 0.35):   
Category A and B joints which respect the condition indicated in UCS-68(b)(1) - e.g. 100%RT.
Lightly loaded attachments (<25% stress value) which respect the condition indicated in UCS-68(b)(2)(-a) 
Seal welds (tube to tube sheet)

 It does not exempt from PWHT the category “C” and “D” joints , and fillet welds (except as defined as “lightly loaded attachments” 

govindan krishnamoorthy

no leída,
23 sept 2020, 1:49:3923/9/20
a material...@googlegroups.com
Since the Code is specifically indicated exemption only  for Category A and B joints. ( I checked for ASME INTREPRATION sheet not found any specific on this query).
Hence , this does not give provisions to take exemption credit for other categories which doesn't indicated in the code specifically. 

Plz provide if u have any latest interpretation if any for further discussion. 


From: material...@googlegroups.com <material...@googlegroups.com> on behalf of MW <raghura...@gmail.com>
Sent: Wednesday, 23 September 2020, 11:06
To: Materials & Welding
Subject: [MW:31500] Re: ASME BPV Sec VIII div1 , UCS-68(b) - PWHT requirements
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/df4bd57b-dfe4-4865-9159-80999d2e474bn%40googlegroups.com.

George Dilintas

no leída,
23 sept 2020, 9:11:0323/9/20
a material...@googlegroups.com
Yes C and D welds are not exempted. most probably because a geometrical discontinuity is always associated with a C and D weld.

There is also an interpretation relevant to UCS-68(b):

Standard Designation:BPV Section VIII Div 1
Edition/Addenda:
Para./Fig./Table No:
Subject Description:Section VIII, Division 1 (1998 Edition, 1999 Addenda); UCS-68(b)
Date Issued:01/14/2000
Record Number:BC99-597
Interpretation Number :VIII-1-98-99
Question(s) and Reply(ies):


Question: Do the requirements of UCS-68(b) in Section VIII, Division 1 apply to tube-to-tubesheet welds?

Reply: Yes.



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/df4bd57b-dfe4-4865-9159-80999d2e474bn%40googlegroups.com.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis