Stabilization heat treatment

48 views
Skip to first unread message

K.M Hrishikesan

unread,
Apr 1, 2021, 11:14:14 PM4/1/21
to materials-welding
Hi..Need a small help.
Does  anybody have an established WPS for stabilization heat treatment?
MOC:
 ASTM A 358 TP 347
Specimen thickness is 25 mm.

Thanks.

Vishwas Keskar

unread,
Apr 1, 2021, 11:27:19 PM4/1/21
to material...@googlegroups.com
Is this Stabilisation is for  Pipe to Pipe butt joint ?



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFHBd__iMawJ0FOuy0xRBiCp3ZHr%2BfhFSjuHgkbP4ZrLM-ndCg%40mail.gmail.com.

K.M Hrishikesan

unread,
Apr 1, 2021, 11:59:19 PM4/1/21
to materials-welding

Vishwas Keskar

unread,
Apr 4, 2021, 10:36:49 PM4/4/21
to material...@googlegroups.com
Hope this SS TYP347 piping job .
 Stabilisation HT shall be as per below HT cycle 
Method of Heat treatment - HT using Electric Resistance Pads  suitable to achieve temperature of 1000  Deg C 
Loading at or below - 200 Deg C 
Rate of Heating - 200  Deg C / hr 
Holding temperature - 920 +/- 10  Deg C 
  Holding time - 125 minutes 
  Rate of Cooling  - Remov Electric Resistance Pads  after holding period is over  - Forced Air cooling - Use  Dry Air Blast   
  Unloading at or below - Room temperature
Note - The job shall be supported suitably to avoid distortion of PIping spools .
attach thermocouple as per Pipe diameter .


Rajnish Dixit

unread,
Apr 12, 2021, 12:55:28 AM4/12/21
to material...@googlegroups.com
Hi,
It is same ordinary WPS like others.
There will be only addition to heat treatment @ 900 degree C for four hours soaking time followed by air quenching (cooling I'm open air). 

Thanks,
--

Vishwas Keskar Welding Manager WELDING

unread,
Apr 13, 2021, 10:25:02 PM4/13/21
to Materials & Welding
As I recall .we had done for 18.26 mm