PQR for PTAW Process by ASME Sec IX

105 views
Skip to first unread message

sathis...@gmail.com

unread,
Sep 22, 2019, 11:24:23 PM9/22/19
to Materials & Welding
Dear Experts I would like to know below query on preparation of PQR as per ASME Sec IX, Process: PTAW by hardfacing overlay by Stellite 6 Powder 1. What is the current, voltage, Gas flow and Powder feed rate need to be maintained for 10mm and 25mm thickness plate. To which standard and reference i need to refer. 2. What is the pre heating and interpass temperature need to be maintained for P.No: 1,8,4,5A, 15E and to which standard need to refer 3. What is the hardness requirement for P.No: 1,8,4,5A, 15E during testing PQR? Which standard is mentioned this requirement? 4. Chemical analysis is mandatory for Co base as per ASME Sec IX , Table QW: 453 Kindly give your suggestion and feedback for the above doubts Thanks in advance

Bien_ND / weldinginspections.net

unread,
Sep 24, 2019, 5:48:10 AM9/24/19
to Materials & Welding
please run follow machine manual and consumable manual.
I did a procedure PTA with Dura-Metal as them instruction.

José Juan Jiménez Alejandro

unread,
Sep 24, 2019, 11:50:01 PM9/24/19
to material...@googlegroups.com
It is important that you mention what the Construction Code is

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/26d6e35c-4e74-4687-a9b1-425343919b7e%40googlegroups.com.


--

Ing. José Juan Jiménez Alejandro

Independent Consultant in Parts

and Pressure Equipment

SSI-TPI

Móvil +52 1 812 352 4606

Skype: jjjimeneza





sathis...@gmail.com

unread,
Oct 3, 2019, 11:07:24 PM10/3/19
to Materials & Welding
Dear Sir
Construction code is API 6A

Kindly clarify below doubt, I have carried out trial welding on 25mm and 10mm test plate size of 170mmX170mm
1. I have carried out macro examination and no indication
2. Chemical analysis done at 1.6mm weld metal. Found Fe content in 10mm plate to 7.85% and 25mm plate 12.58%. Kindly clarify whether it is acceptable? do i need to check the chemical as per the filler wire composition? also normally dilution will not be controlled and Fe is observed above the spec

What is the acceptable limit?

3. As per the ASME Sec IX i have carried out 3 hardness at weld metal of 1.6mm as same as chemical test piece sample. Or do i need to check at the weld interface of weld metal, HAZ and base metal? kindly clarify

please give us the valuable inputs


On Wednesday, September 25, 2019 at 9:20:01 AM UTC+5:30, José Juan Jiménez Alejandro wrote:
It is important that you mention what the Construction Code is

El mar., 24 sept. 2019 a las 4:48, Bien_ND / weldinginspections.net (<bck...@gmail.com>) escribió:
please run follow machine manual and consumable manual.
I did a procedure PTA with Dura-Metal as them instruction.


On Monday, September 23, 2019 at 10:24:23 AM UTC+7, sathis...@gmail.com wrote:
> Dear Experts
>
> I would like to know below query on preparation of PQR as per ASME Sec IX, Process: PTAW by hardfacing overlay by Stellite 6 Powder
>
>
>
> 1. What is the current, voltage, Gas flow and Powder feed rate need to be maintained for 10mm and 25mm thickness plate. To which standard and reference i need to refer.
>
>
>
> 2. What is the pre heating and interpass temperature need to be maintained for P.No: 1,8,4,5A, 15E and to which standard need to refer
>
>
>
> 3. What is the hardness requirement for P.No: 1,8,4,5A, 15E during testing PQR? Which standard is mentioned this requirement?
>
>
>
> 4. Chemical analysis is mandatory for Co base as per ASME Sec IX , Table QW: 453
>
>
>
> Kindly give your suggestion and feedback for the above doubts
>
>
>
> Thanks in advance

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
Reply all
Reply to author
Forward
0 new messages