Carbon/Manganese pressure vessel ASME VIII, Crack after PWHT

54 views
Skip to first unread message

Zakaria ghrab

unread,
Apr 6, 2016, 10:48:56 PM4/6/16
to material...@googlegroups.com
Dear Experts,

 Need your support for one issue :

Construction code : ASME VIII Div 1
Pressure vessel fabrication.
Material: A516 Gr 70N
Thickness : 48 mm
Welding process : SAW/FCAW;
Joint design: X

For one of Circulaire joints, UT & TOFD performed before PWHT and result was conform.
After PWHT, One crack around 40mm lenght, detected centerline of the weld surface in the internal side of vessel.

In my assessment, 

  • crack may be hydrogen crack dur to no control of interpass temperature and heat input or due to Carbon picked up from parent metal to weld zone and due to lower manganese concentration, Crack occurs.
  • May be Crack taked time to occurs (it's possible that crack present after 03 days of weldment, please confirm to us) and in this case may be NDE performed before crack that's why NDE reports before PWHT present conform result.

Please your support & Feedback experience and what you propose as corrective / Preventive actions.


--

Thanks and Regards, ?
-----
زكرياء غراب
GHRAB Zakaria 
EA2C Tunisia.
Tunisia : +216 96 635 805
Bénin : +229 97 128 387


Yesterday is the past, tomorrow is the future; and today? Today is the present, the gift: Enjoy it!

Mohd Siraj

unread,
Apr 8, 2016, 12:15:38 AM4/8/16
to Materials & Welding
Whts exactly joint geometry?
top and bottom bevel thk?

is it equal??

or unequal??

whts filer metal??

is joint well supported from both end??

did u used crushed flux??

flux was preheated??

How you hve filled groove top full complete after other side..??


dili...@gmail.com

unread,
Apr 17, 2016, 10:49:24 AM4/17/16
to Zakaria ghrab
Most probably cold cracking. Hydrogen bake out treatment should have been implemented.

Sent from my BlackBerry 10 smartphone.
From: Zakaria ghrab
Sent: Πέμπτη, 7 Απριλίου 2016 - 05:48
Subject: [MW:24636] Carbon/Manganese pressure vessel ASME VIII, Crack after PWHT

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAD8EeB21thvysyFQ3zyYybv0MquE8WanbnjW-W%3Dcpp7DE2vUaw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Kannayeram Gnanapandithan

unread,
Apr 18, 2016, 1:24:43 AM4/18/16
to materials-welding

Centre of weld is not due to Hydrogen. Improper cleaning & impurities which was relaxed after PWHT

--