Re: [MW:0] Welding of CS+Alloy825 clad pipies

184 views
Skip to first unread message

B.Vaithiyanathan

unread,
Jul 8, 2010, 11:13:32 AM7/8/10
to materials-welding
Hi 
       The Consumable for your case is ER NiCrMo3/E NiCrMo3

Regards,
Vaithiyanathan

On Thu, Jul 8, 2010 at 2:52 PM, romio dabre <romio...@gmail.com> wrote:
Dear All
 
We have to weld 20" to 36" pipe spools with following details. Joints cannot be backwelded or cannot do clad restoration from inside.
Material CS+Alloy 825 clad
Thk between 20mm to 54mm
Complete weld with Alloy 625 will be very costly as the thk is high.
What will be the recommended welding consumable combination.
 
Thnaks
 

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
With Best Regards

B.Vaithiyanathan

pgoswami

unread,
Jul 10, 2010, 1:44:35 PM7/10/10
to material...@googlegroups.com
Hi Romiomdabre,
 
The default technique for such pipe spool (where welding from I/S is not possible) would be to use Inconel-625(E/ER-NiCrMo-3) fillers and electrodes all through. Yes this would make  cost of welding quite high. As you know these piping are exposed for extremely harsh service environments, proven welding consumables are required to meet the design and construction and service requirements. Typical offshore pipeline design specifications such as DNV-OS-F-101 indicates one "type" of welding consumable for single sides welding of clad pipes.
 
I would think there are  some alternatives practiced in the industry,  in the way of using Stainless/ Nickel Based alloys for clad welding + application a pure Iron barrier layer on the clad weld followed by welding with C.S electrodes on C.S base metal. The attached extract of 10064-Page2(15) Fig-26 shows the welding sequences. While this technique has been proven for welding of S.S clad C.S pipes, there had not been much information available on the same for welding of Inconel Clad pipes. The critical factors here is the availability of Pure Iron electrode and acceptance of the same by fabrication code. A sample from Lincoln Electric is attached for information.If any other forum members could shed some lights on this issue,it would be appreciated.
 
Incidentally similar query was raised in another forum,few years ago.I have attached the responses and discussions for
 
Thanks
 
Pradip Goswami,P.Eng.
Welding & Metallurgical Engineer/Specialist
Ontario Power Generation Inc.
Email-pgoswami@sympatico.ca,
 


From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of B.Vaithiyanathan
Sent: Thursday, July 08, 2010 11:14 AM
To: materials-welding
Subject: Re: [MW:5904] Welding of CS+Alloy825 clad pipies

10064-Engineering with Clad Steels-Extract.pdf
Kardo-Lincoln.pdf
DNV-OS-F-101-Submarine Pipelines-Extract.pdf
Clad pipe to Clad pipe Welding.pdf

james gerald

unread,
Jul 11, 2010, 6:59:33 AM7/11/10
to material...@googlegroups.com
Hi Goswami,
 
What is the PQR requirement for this joint. Does it need to comply with QW217(a) of ASME Sec.iX. Is any chemical analysis required.

J.GERALD JAYAKUMAR
00919344954677
 


--- On Sat, 7/10/10, pgoswami <pgos...@quickclic.net> wrote:

HUY HOÀNG

unread,
Mar 10, 2025, 11:58:37 PM3/10/25
to Materials & Welding
HI SIR
I use E309 or E310 for buttering layers. Is it correct ?
I use ernicrmo-3 for root, hot, f1, f2 
then i use E309 in 2 layers
Completely with k7018 to the end. 
It can or can not do it?
Thank you for answering me.
Hope u have a great day

Vào lúc 00:44:35 UTC+7 ngày Chủ Nhật, 11 tháng 7, 2010, pgoswami đã viết:

Noman Ahmed

unread,
Mar 11, 2025, 11:18:25 PM3/11/25
to material...@googlegroups.com
Dear Sir,
            does somebody share the latest CSWIP 3.1 exam questions with new pattern?

regards,
noman

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/c8dd9575-7444-4541-bc34-abe1c8efaec2n%40googlegroups.com.
Reply all
Reply to author
Forward
0 new messages