API 650 Bottom Plate Distortion

127 views
Skip to first unread message

Abd Ur Rehman

unread,
May 25, 2024, 1:36:14 AM5/25/24
to Materials & Welding
Hello everyone hope u all be fine 
my question is that , as per ur experince how much API 650 Bottom Plate Distortion is acceptable .

Anand ch

unread,
May 29, 2024, 3:12:01 AM5/29/24
to Materials & Welding
Dear Abd Ur Rehman,

Out-of-plane distortion equal to 1 percent of the tank radius is considered acceptable."
While that's not an API requirement, that should be a measure of industry standard, 
and that plate distraction not affected on length of the plate that is acceptable range means it will accept the bottom plate 

Abd Ur Rehman

unread,
Jun 6, 2024, 5:52:12 AM6/6/24
to material...@googlegroups.com
how much tolerance is acceptable in circumference (API650) storage tanks.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b4bfa48a-a6f2-4dc8-b271-1588e463b79fn%40googlegroups.com.

agum...@gmail.com

unread,
Jun 7, 2024, 2:20:00 PM6/7/24
to Materials & Welding
Hello it depend of tank diameter:

API 650 2021  7.5. Roundness

 

Radii measured at 0.3 m (1 ft) above the bottom corner weld shall not exceed the following tolerances:


Tank Diameter m (ft)


Radius Tolerance mm (in.)


< 12 (40)                                                                              ± 13 (1/2)

From 12 (40) to < 45 (150)                                                   ± 19 (3/4

From 45 (150) to < 75 (250)                                                  ± 25 (1)

75 (250)                                                                           ± 32 (11/4)

Mohd Siraj

unread,
Jun 12, 2024, 11:28:52 AM6/12/24
to Materials & Welding
50mm acceptable, lets know if it tank is in service?, refer api 653., by the way bottom plate distortion refer as settlement, better to refer with correct terminology.