TESTS REQUIRED FOR PQR OF CORNER JOINT WITH SINGLE GROOVE WELD

229 views
Skip to first unread message

vikas shelke

unread,
May 7, 2015, 1:08:02 PM5/7/15
to material...@googlegroups.com
Hello everyone,
    I have to qualify EN3A Plate to SA 106 Gr B Pipe Corner joint with single J Groove outside
Inline image 1.
Will you please suggest the TESTS required for the qualification of Procedure as per ASME Sec IX;
    

--
 
 Regards,

   Vikas 


george....@gr.bureauveritas.com

unread,
May 7, 2015, 10:21:27 PM5/7/15
to vikas shelke
This qualifies as a butt joint

Sent from my BlackBerry 10 smartphone.
From: vikas shelke
Sent: Πέμπτη, 7 Μαΐου 2015 - 20:08
Subject: [MW:23229] TESTS REQUIRED FOR PQR OF CORNER JOINT WITH SINGLE GROOVE WELD

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALmPzdUGSyoZAkzZS51h3S5Q2CkwXzYEUh-rih%3Df%3DgtUFzTE2A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

vikas shelke

unread,
May 8, 2015, 4:04:34 AM5/8/15
to material...@googlegroups.com
but How test specimens for Tensile tests will be drawn as the pipe thickness is 12 mm & Plate thickness is 30 mm?


For more options, visit https://groups.google.com/d/optout.



--
 
 Regards,

Vikas Shelke,

+91-9881749268.

george....@gr.bureauveritas.com

unread,
May 8, 2015, 5:56:50 AM5/8/15
to material...@googlegroups.com

You do not need to make a mock -up.
Just take select two pieces of plates by respecting all essential and supplementary essential variables (if impact test is required).
The form of bevel and the diameter are not essential variables for ASME BPVC Section IX

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


Inactive hide details for vikas shelke ---08/05/2015 11:04:37---but How test specimens for Tensile tests will be drawn as the pvikas shelke ---08/05/2015 11:04:37---but How test specimens for Tensile tests will be drawn as the pipe thickness is 12 mm & Plate thickn



From: vikas shelke <vikas.s...@gmail.com>
To: material...@googlegroups.com
Date: 08/05/2015 11:04
Subject: Re: [MW:23232] TESTS REQUIRED FOR PQR OF CORNER JOINT WITH SINGLE GROOVE WELD
Sent by: material...@googlegroups.com





but How test specimens for Tensile tests will be drawn as the pipe thickness is 12 mm & Plate thickness is 30 mm?

On Fri, May 8, 2015 at 7:51 AM, <george....@gr.bureauveritas.com> wrote:

    This qualifies as a butt joint

    Sent from my BlackBerry 10 smartphone.

    Hello everyone,
        I have to qualify EN3A Plate to SA 106 Gr B Pipe Corner joint with single J Groove outside

chirag...@gmail.com

unread,
May 9, 2015, 12:24:02 AM5/9/15
to material...@googlegroups.com
Dear sir,

If you are using wps for corner joint for box type header for air cooled heat exchangers. Refer mandatory appendix 28 of ASME sec VIII-1.

Regards,
Chirag patel

Sent from my BlackBerry 10 smartphone.
Sent: Friday 8 May 2015 3:26 PM
Subject: Re: [MW:23234] TESTS REQUIRED FOR PQR OF CORNER JOINT WITH SINGLE GROOVE WELD

vikas shelke

unread,
May 9, 2015, 12:24:20 AM5/9/15
to material...@googlegroups.com
Thank you sir, I think I got the point , (kindly correct me if I am wrong for the following); 
So I will take the EN3A plate & P1GR1 Plate Material (as impact test is there) for welding and carry out the qualification.


For more options, visit https://groups.google.com/d/optout.

Muhammed Ibrahim PK

unread,
May 9, 2015, 2:27:27 AM5/9/15
to material...@googlegroups.com
For sec IX it is not required. For AWS D 1.1 it is required.

Thanks & Regards
Muhammed Ibrahim PK

george....@gr.bureauveritas.com

unread,
May 9, 2015, 1:59:10 PM5/9/15
to vikas shelke
Correct just match all essential and supplementary essential variables

Sent from my BlackBerry 10 smartphone.
From: vikas shelke
Sent: Σάββατο, 9 Μαΐου 2015 - 07:24
Subject: Re: [MW:23240] TESTS REQUIRED FOR PQR OF CORNER JOINT WITH SINGLE GROOVE WELD


For more options, visit https://groups.google.com/d/optout.