Dear Sir,

 We conducted welder qualification at Karbala Oil Refinery Project as per ASME-IX 2013 Edition. 

 WPS details as follow 
1. WPS qualified base metal- P1 to P1 Gruop all
2. WPS mentioned base metal thickness range- 5 to 26 mm
3. Process FCAW
WQT details
1. Joint design Single V butt joint with back weld(Root side back grind then weld)
2. Base metal SA283-C
3. Thickness 16.0 mm
4. Sequence of welding- Root pass>Hot Pass>Filling>Capping>Back grind & Back weld
5. Test position 2G & 3G 

My client inspector say welder will qualified only for 2T  & Pipe Diameter will qualify over 24" I want to clarify is he correct? For thickness qualified he mention about QW-404.30 
However I will appreciate to you for clarify my problem.




Regards
Anamul
QA/QC Engineer


Dharmendra KL

unread,
Jan 18, 2016, 11:01:08 PM1/18/16
to material...@googlegroups.com
Maximum thickness he can weld as per 452.1b
Pipe OD from 73dia to above 24inch he can weld with limitations as per 461.9

From: anam...@gmail.com
Sent: ‎19-‎01-‎2016 07:55
To: Materials & Welding
Subject: [MW:24126] Qualified thickness for welder

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b86d11c7-1ff9-4ee6-b63e-040e6aafcdbe%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Padmasanker S

unread,
Jan 19, 2016, 12:42:36 AM1/19/16
to material...@googlegroups.com

Hi Mr Anamul,

For qualification mentioned in below mail ,thickness qualified is unlimited. Refer para QW-452.1b.
Note that Para QW-404.30 cross refers para QW-452.1b for performance qualification by radiography.
For position qualification refer para QW-461.9.
The welder is qualified to weld flat position for size less than or equal to 24" pipes and flat & vertical position in size more than 24" pipes.

hope this clarifies you.

Best regards,

Padmasanker.s
Project quality coordinator,
Bilfal heavy industries ltd.

afrozsh...@gmail.com

unread,
Jan 19, 2016, 8:31:21 AM1/19/16
to Materials & Welding
Dear Anamul,

I had checked and agreed with Mr. Padmashankar comments, pls go ahead for discussion with client inspector.

Regards,
Afroz Shaikh
IOTIES

george....@gr.bureauveritas.com

unread,
Jan 29, 2016, 5:05:00 AM1/29/16
to material...@googlegroups.com

I the deposited thickness was 13 mm and over and he has deposited at least 3 layers then the range is not  2t but the maximum to be welded (restricted by the WPS)
best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS HELLAS A.E  - PIRAEUS  GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


Inactive hide details for anamulqc---19/01/2016 04:25:18---Dear Sir,  We conducted welder qualification at Karbala Oil Refineryanamulqc---19/01/2016 04:25:18---Dear Sir,  We conducted welder qualification at Karbala Oil Refinery Project as per



From: anam...@gmail.com
To: Materials & Welding <material...@googlegroups.com>
Date: 19/01/2016 04:25
Subject: [MW:24126] Qualified thickness for welder

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-weld...@googlegroups.com.
To post to this group, send email to
material...@googlegroups.com.
Visit this group at
https://groups.google.com/group/materials-welding.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/b86d11c7-1ff9-4ee6-b63e-040e6aafcdbe%40googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Asif Raza

unread,
Jan 31, 2016, 9:35:26 AM1/31/16
to material...@googlegroups.com
image001.gif

Naresh Kumar

unread,
Feb 1, 2016, 2:16:48 AM2/1/16
to Materials & Welding
Dear Mr.Anamul

Asper ASME SEC-IX-
 
·         Thickness qualified- Unlimited, if the deposited weld metal was at least 3 layers.(according to WPS)
·         Plate and Pipe over 24 in. qualified for F,H & V positions.
·         Pipe qualified of 2 7/8 in.(73 mm) for F & H positions.
·         Only qualified for with backing.
 
 
 
Thanks & Regards
Nareshkumar Subramanian




From: Asif Raza <asif...@yascotech.com>
To: material...@googlegroups.com
Sent: Sunday, January 31, 2016 6:23 PM
Subject: RE: [MW:24195] Qualified thickness for welder

Reply all
Reply to author
Forward
0 new messages