Mahmood Al-Hinai

non lue,
21 mai 2023, 23:10:1521/05/2023
à material...@googlegroups.com
Dear all experts,

If Low Hydrogen Electrods kept directly in a holding oven without backing, and later on it was observed, so how to rectify?
Shall be scraped or backed?


Vishwas Keskar

non lue,
21 mai 2023, 23:47:1321/05/2023
à material...@googlegroups.com
The question is not clear 
Pl elaborate the query

Sent from my iPhone

On 22-May-2023, at 8:40 AM, Mahmood Al-Hinai <hyna...@gmail.com> wrote:


Dear all experts,

If Low Hydrogen Electrods kept directly in a holding oven without backing, and later on it was observed, so how to rectify?
Shall be scraped or backed?


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEuX%2Bd%3D-LvqWgQ-qVC0KqtfcVEP8_haQFEHEK%2BqSw87Ss8ms%3Dg%40mail.gmail.com.

Mahmood Al-Hinai

non lue,
22 mai 2023, 01:15:0822/05/2023
à material...@googlegroups.com
As you know, Low hydrogen Electrods shall be baked (350 degree for 2 hours), but in this case the workshop supervisor didn't bake them, instead of that, he kept them directly in holding oven. 

So shall these electrods scrapped or baked and used? 

Baqer Shabbeer

non lue,
22 mai 2023, 01:15:0922/05/2023
à material...@googlegroups.com

 

Hi, Good day,

 

When it comes to baking, you need to maintain the backing oven temperature 260-430 degrees Celsius. While maintaining a temperature of 120 degrees Celsius is for holding purposes,. At 120 degrees Celsius, the flux coating does not experience any significant heat impact, which can’t potentially lead to flux damage, baking requires a higher range of 260-430 degrees Celsius.

Considering the above statement you can go for baking.

Vishwas Keskar

non lue,
22 mai 2023, 04:39:5122/05/2023
à material...@googlegroups.com

Pl get the electrodes back to  Stores
Identify these by AWS name.
Segregate fully intact flux covered electrodes 

Carry out baking as per Consumable Mfg  recommendation
After baking is completed transfer to Holding oven 

issue to Production as per  Consumable Slip Request as required

Make a record in baking  , Holding register 

Thanks 
Vishwas - IWE 


Sent from my iPhone