PT inspection after Grinding a Weld Seam?

42 views
Skip to first unread message

Mohamed Arbaoui

unread,
Jun 26, 2025, 12:55:00 PM6/26/25
to material...@googlegroups.com

Dear Members,

I have a question since I'm a beginner in this domain.


After a weld inspection by PAUT, a crack was detected at a certain depth. I noticed that the welders grind down the weld surface until they reach the depth indicated by PAUT, and then apply a PT test.
My concern is: isn't there a risk that the grinding process may partially close or smear the crack surface, making it harder for the PT liquid to penetrate and properly reveal the defect?

If so, this could mean that PT might give a false result, and the crack would only be detected later when PAUT is reapplied after re-welding.

Am I misunderstanding the procedure? What is the best practice in this case?

Thanks,

sridhar cn

unread,
Jun 27, 2025, 4:04:17 AM6/27/25
to material...@googlegroups.com


Your concern is valid. Grinding a weld surface down to the depth indicated by PAUT before performing a Penetrant Test (PT) can indeed

risk smearing or partially closing the crack surface. Grinding down to the PAUT-indicated crack depth before PT can cause smearing that 

partially closes cracks, making PT less effective and potentially leading to false negatives.

To avoid this:

Use a low force (a lower grind pressure) and avoid overheating during final grinding to minimise smearing. Employing the bleed-back 

technique (i.e., after applying developer in PT, wiping the area and reapplying developer can help reveal cracks if there is still an open path 

to the surface. If the indication reappears, further light grinding may be needed to reopen cracks before performing the PT. Interpret PT 

results with caution after grinding and confirm with ultrasonic methods if needed. 

This combined approach ensures more reliable detection of weld cracks and reduces the risk of missing critical defects. 

C Sridhar.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAPkLCPCL2hOdFw0rDsd9TnRf60vC7YDwYhFib8g%2BujNVkSDerg%40mail.gmail.com.
Reply all
Reply to author
Forward
0 new messages