Dear Expert,

I am having 2 PQRs i.e.:
1. 2" Sch. 80 Pipe (thk.-5.54mm) - GTAW (70S-2)
2. 6" Sch. 160 Pipe (thk.-18.26mm) - SMAW (7018)

My question is: Can I combine these 2 PQRs for buiding up one more making new WPS for 8" Sch. 80 Pipe (thk.-12.70mm) using GTAW+SMAW (Root and hot with GTAW and filling and capping with SMAW)

Thanx in advance

John Henning

unread,
Jan 17, 2017, 11:35:28 AM1/17/17
to material...@googlegroups.com

NO - Per ASME IX.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c48bcc22-b50c-4d5a-8147-e4a0c3a3db39%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

hajarath ali

unread,
Jan 18, 2017, 12:28:34 AM1/18/17
to Materials & Welding
Alternative is prepare two WPS and use it in a single production joint combination of WPS is applicable ...
Reference ASME SEC IX QW 200.4

Manoj Singh

unread,
Jan 18, 2017, 10:24:39 AM1/18/17
to material...@googlegroups.com

Yes u can pls.refer sec Ix welding general requirement.

On 17 Jan 2017 9:35 pm, "John Henning" <jhen...@deltak.com> wrote:

NO - Per ASME IX.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Lalit Malla
Sent: Tuesday, January 17, 2017 6:07 AM
To: Materials & Welding
Subject: [MW:25915] Combining 2 PQRS

 

Dear Expert,

 

I am having 2 PQRs i.e.:

1. 2" Sch. 80 Pipe (thk.-5.54mm) - GTAW (70S-2)

2. 6" Sch. 160 Pipe (thk.-18.26mm) - SMAW (7018)

 

My question is: Can I combine these 2 PQRs for buiding up one more making new WPS for 8" Sch. 80 Pipe (thk.-12.70mm) using GTAW+SMAW (Root and hot with GTAW and filling and capping with SMAW)

 

Thanx in advance

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/MWHPR03MB28167C7A015E4BD1CA3AEB91A17C0%40MWHPR03MB2816.namprd03.prod.outlook.com.

prashant pansare

unread,
Jan 18, 2017, 10:54:52 AM1/18/17
to material...@googlegroups.com
Check qualification limit for dia as per Sec IX.

--

John Henning

unread,
Jan 18, 2017, 11:47:43 AM1/18/17
to material...@googlegroups.com

Note:

 

Diameter is not an essential or non-essential variable for procedure qualification.

 

Diameter is an essential variable for weldor performance qualification.

 

Therefore not applicable to the question.

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of prashant pansare
Sent: Wednesday, January 18, 2017 9:51 AM
To: material...@googlegroups.com
Subject: Re: [MW:25932] Combining 2 PQRS

 

Check qualification limit for dia as per Sec IX.

On Jan 17, 2017 6:00 PM, "Lalit Malla" <lalit...@gmail.com> wrote:

Dear Expert,

 

I am having 2 PQRs i.e.:

1. 2" Sch. 80 Pipe (thk.-5.54mm) - GTAW (70S-2)

2. 6" Sch. 160 Pipe (thk.-18.26mm) - SMAW (7018)

 

My question is: Can I combine these 2 PQRs for buiding up one more making new WPS for 8" Sch. 80 Pipe (thk.-12.70mm) using GTAW+SMAW (Root and hot with GTAW and filling and capping with SMAW)

 

Thanx in advance

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFw%3DPEhga7Jo%2BWUMOgq5bcSw-K%2BTPfVvdCj7_sAGqib8X5aLPQ%40mail.gmail.com.

John Henning

unread,
Jan 18, 2017, 11:52:30 AM1/18/17
to material...@googlegroups.com

Yes you can combine them. 

 

NO it will not meet his requirements as you will be limited to the qualification thicknesses for base metal and weld metal of the GTAW process.  See QW-200.4(a)(1) and QW-200.4(a)(2).  His combined weld cannot be greater than 2T and 2t for the GTAW -  i.e. 11.04mm for both.  Thus, the root cannot be made on the 12.70mm thick weld.

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Manoj Singh
Sent: Wednesday, January 18, 2017 1:09 AM
To: material...@googlegroups.com
Subject: RE: [MW:25924] Combining 2 PQRS

 

Yes u can pls.refer sec Ix welding general requirement.

On 17 Jan 2017 9:35 pm, "John Henning" <jhen...@deltak.com> wrote:

NO - Per ASME IX.

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Lalit Malla
Sent: Tuesday, January 17, 2017 6:07 AM
To: Materials & Welding
Subject: [MW:25915] Combining 2 PQRS

 

Dear Expert,

 

I am having 2 PQRs i.e.:

1. 2" Sch. 80 Pipe (thk.-5.54mm) - GTAW (70S-2)

2. 6" Sch. 160 Pipe (thk.-18.26mm) - SMAW (7018)

 

My question is: Can I combine these 2 PQRs for buiding up one more making new WPS for 8" Sch. 80 Pipe (thk.-12.70mm) using GTAW+SMAW (Root and hot with GTAW and filling and capping with SMAW)

 

Thanx in advance

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPkJdRKm7zjORZR5%2BbquvLEO%3DV%2BWOmGNBqWNTZt2dgMXV0TTMA%40mail.gmail.com.

dilintas

unread,
Jan 19, 2017, 5:52:12 AM1/19/17
to material...@googlegroups.com
Diameter is not a qualifying variable in ASME IX



Sent from my Samsung Galaxy smartphone.

-------- Original message --------
From: prashant pansare <prashan...@gmail.com>
Date: 18/01/2017 17:50 (GMT+02:00)
Subject: Re: [MW:25932] Combining 2 PQRS

Check qualification limit for dia as per Sec IX.
On Jan 17, 2017 6:00 PM, "Lalit Malla" <lalit...@gmail.com> wrote:
Dear Expert,

I am having 2 PQRs i.e.:
1. 2" Sch. 80 Pipe (thk.-5.54mm) - GTAW (70S-2)
2. 6" Sch. 160 Pipe (thk.-18.26mm) - SMAW (7018)

My question is: Can I combine these 2 PQRs for buiding up one more making new WPS for 8" Sch. 80 Pipe (thk.-12.70mm) using GTAW+SMAW (Root and hot with GTAW and filling and capping with SMAW)

Thanx in advance

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

Ahmed Elgendy

unread,
Oct 26, 2019, 1:11:49 AM10/26/19
to material...@googlegroups.com
Dear experts
is there any WPS for welding cast iron plate 29 cm thickness
regards,

Souravbohray

unread,
Oct 28, 2019, 5:32:40 AM10/28/19
to Materials & Welding
Mr John is right please reffer qw2004. B sec9
Reply all
Reply to author
Forward
0 new messages