suresh

unread,
Nov 10, 2015, 2:38:38 AM11/10/15
to material...@googlegroups.com
Dear Experts

Requesting to share your valuable experience regarding welding of high pressure mud gate valve (ASTM A 487 Gr A Class 4) to Seamless pipe (JIS G 3455 STS-42)
 
I would like to know the suitable consumables for SMAW process and preheating and PWHT temperature if applicable.

Best Regards,
NDB Suresh,


Morteza Derikvandi

unread,
Jan 15, 2017, 11:42:32 PM1/15/17
to Materials & Welding
Hi mate
It seems a bit late to answer :)
But it's better that question be answered.

USE E 8018-B2
Minimum Pre-Heat Temperature: 95 °C (Use 150 °C as
Default & Dont let it reach below 120 °C during welding)
PWHT  must be at or below the final tempering temperature : 595
°C