Dear Experts
Good day!!!

I'll highly appreciated if you share your valuable ideas regarding reason for difference between Cr content range in A351 CF8M and A182F316 which is 18-21% and 16-18% respectively.

Regards,
H.Nikdin

George Dilintas

unread,
Aug 23, 2016, 9:24:26 AM8/23/16
to Meghanadh K
not only Cr is higher but also Ni is lower. 


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BLU405-EAS243C25FF6CC7E1A871214F39EE80%40phx.gbl.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

Himan Nikdin

unread,
Aug 23, 2016, 9:44:36 AM8/23/16
to material...@googlegroups.com
Would you please for the reason?

Sent from my iPhone
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40DFsi6F7Uj2JJsS7a5JGLyoTdqP3D_yjFX7eEW-oy4wsQ%40mail.gmail.com.

pgoswami

unread,
Aug 23, 2016, 11:02:21 AM8/23/16
to material...@googlegroups.com

Castings are manufactured by “Melting & pouring “Technique. Alloy losses are more in during casting; hence the compositional range is wider.

Materials chosen for forging already will have some preset compositions, not the same as casting where the composition is to be finalized, when the liquid metal is to be poured. Hence the range could be narrower.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,

Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

H-905-6799677, 905-9631505

C-905-9793232

 


To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BLU405-EAS244572849CDE9ACC115CFF9EEB0%40phx.gbl.

Himan Nikdin

unread,
Aug 24, 2016, 2:00:40 AM8/24/16
to material...@googlegroups.com
Dear Pradip

Please note that the issue is not narrower or wider composition range but is the reason for acceptable level of Cr,Ni.
I found that stainless steel castings require delta ferrite for strengthening because there is no way to hot work or heat treatment to increase strength level, so increasing Cr and decreasing Ni level promotes delta ferrite.
Actually austenitic stainless steel castings have duplex structure, also delta ferrite has adverse effects on forgeability of stainless steels and limits forging temperature (but I don't know what is adverse effect and how much temperature limit), so delta ferrite should be limited in forgings by decrease Cr level and increase Ni level to decrease delta ferrite. 
In the meantime I found that delta ferrite increase weld ability of castings, would you please let me know how and why?


Regards,
Himan Nikdin

Sent from my iPhone

Kannayeram Gnanapandithan

unread,
Aug 24, 2016, 3:27:18 AM8/24/16
to materials-welding

Delta ferrite reduce ductility and mechanical properties. What Pradeep explained is the manufacturing scenario.


On 24-Aug-2016 11:30 am, "Himan Nikdin" <himan....@outlook.com> wrote:
Dear Pradip

Please note that the issue is not narrower or wider composition range but is the reason for acceptable level of Cr,Ni.
I found that stainless steel castings require delta ferrite for strengthening because there is no way to hot work or heat treatment to increase strength level, so increasing Cr and decreasing Ni level promotes delta ferrite.
Actually austenitic stainless steel castings have duplex structure, also delta ferrite has adverse effects on forgeability of stainless steels and limits forging temperature (but I don't know what is adverse effect and how much temperature limit), so delta ferrite should be limited in forgings by decrease Cr level and increase Ni level to decrease delta ferrite. 
In the meantime I found that delta ferrite increase weld ability of castings, would you please let me know how and why?


Regards,
Himan Nikdin

Sent from my iPhone

On Aug 23, 2016, at 19:32, pgoswami <pgos...@quickclic.net> wrote:

Castings are manufactured by “Melting & pouring “Technique. Alloy losses are more in during casting; hence the compositional range is wider.

Materials chosen for forging already will have some preset compositions, not the same as casting where the composition is to be finalized, when the liquid metal is to be poured. Hence the range could be narrower.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,

Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

H-905-6799677, 905-9631505

C-905-9793232

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BLU405-EAS244572849CDE9ACC115CFF9EEB0%40phx.gbl.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Reply all
Reply to author
Forward
0 new messages