SA335 P91 to SA106Gr.B Dissimilar Material Welding Procedure

199 views
Skip to first unread message

Vijay Kumar

unread,
Sep 16, 2024, 3:37:39 AM9/16/24
to Materials & Welding
Dear Experts,

I need SA335 P91 to SA106Gr.B Dissimilar Material Welding Procedure with some reference codes. 

Please share 

Thanks 
Vijayakumar

Raviraj Gohil

unread,
Sep 16, 2024, 4:41:03 AM9/16/24
to material...@googlegroups.com
Dear Vijay Kumar,

Please refer API RP 582 , Table A.1

Thanks & Regards,

 

Raviraj Gohil | Manager - Welding | + 83473 02025 | www.lloydsengg.in 




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/be7e26e6-2446-4b69-8ed4-d10c5a074dcfn%40googlegroups.com.

Vishwas Keskar

unread,
Sep 16, 2024, 5:31:43 AM9/16/24
to material...@googlegroups.com
This is not a compatible joint configuration 

Add Gr 22 , Gr 11 stub piece  (150 mm long each )as below .

Gr 91 to Gr 22  - 
Gr 22 to Gr 11 
Gr 11 to CS 

Sent from my iPhone

On 16 Sep 2024, at 2:10 PM, Raviraj Gohil <ravira...@lloyds.in> wrote:



venkateswara reddy Desireddy

unread,
Sep 16, 2024, 7:12:27 AM9/16/24
to material...@googlegroups.com
P91to P1 not correct combination, because of PWHT temperature are different.
Better to do P91 to P22 .


--

Kannayeram Gnanapandithan

unread,
Sep 17, 2024, 12:03:38 PM9/17/24
to material...@googlegroups.com
Not advisable due to lower critical temp of CS is around 725 celsius whereas PWHT heat treatment temp for 91 is around 745 to 760 which will affect the properties of CS
Go with Mr Keskar recomondation.

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Mon, Sep 16, 2024 at 1:07 PM Vijay Kumar <vija...@gmail.com> wrote:
--

Macario Jr. Palola

unread,
Sep 17, 2024, 10:47:16 PM9/17/24
to material...@googlegroups.com
use buttering


The information contained in this email is intended for use only by the recipient to whom or which this is addressed. Such information may be privileged, confidential, and/or proprietary subject to the GMEC Email Disclaimer. Moreover, as we value your privacy, we will handle and safeguard any personal data we receive in this email in accordance with our Privacy Notice.

sridhar cn

unread,
Sep 19, 2024, 11:45:11 AM9/19/24
to material...@googlegroups.com
Mr. Vijay,
Welding P91 to P1 requires careful consideration. due to differences in their thermal 
and mechanical properties. However you can try with:
a proper edge preparation and alignment (to avoid cracks during welding),
using E 9018-B9 /ER90S-B9 filler metals (GTAW is preferred) which are compatible,
preheat to 150-200deg. C throughout to reduce the risk of cracking during welding,
maintain an interpass temp. below 250 deg. C to minimise thermal stresses and 
avoid embrittlement of weld area.
maintain Argon purging throughout, use nominal current to avoid distortion & 
cracking in P91 material
PWHT at 730-800 deg C with proper holding and to relieve stresses,
allow controlled cooling to avoid embrittlement,
monitor for Carbon migration from P1 to P91 which will affect mechanical properties.

In a nutshell, careful adjustments in heat input, preheating & interpass temp. control, and 
PWHT are necessary to ensure a successful welding and maintaining structural integrity.
rgds,
Sridhar.






--

Kannayeram Gnanapandithan

unread,
Sep 20, 2024, 12:13:47 AM9/20/24
to material...@googlegroups.com
not at all advisable to weld P1 directly with P91
Any thing can be welded but what is the metallurgical effect on properties of the weldments. ( Lower Critical temp for P1 material is 725 Celsius)

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

Vinay

unread,
Sep 22, 2024, 11:43:38 AM9/22/24
to material...@googlegroups.com, vijay lemsa Tuti
Dear Friend :
Its not  a recommended combination. But can you please  describe its application? 

On Mon, 16 Sept 2024 at 13:07, Vijay Kumar <vija...@gmail.com> wrote:
--

Md Usman Ghani

unread,
Sep 23, 2024, 6:38:00 AM9/23/24
to material...@googlegroups.com

Which fillers have to use for P91-P22, nd P22-P11 , P11-106


Vishwas Keskar

unread,
Sep 23, 2024, 6:43:43 AM9/23/24
to material...@googlegroups.com
P91 - P22 - TYP B91 /B3
P22 -P11- TYP B3/B2
P11-SA 106 - B2/ Carbon steel 

Normally Higher alloy of the consumables
Deployed 

You can decided based on PQR 
Vishwas-IWE
9823472273
Sent from my iPhone

On 23 Sep 2024, at 4:07 PM, Md Usman Ghani <mdushm...@gmail.com> wrote:



Mohd Siraj

unread,
Oct 5, 2024, 12:44:02 PM10/5/24
to Materials & Welding
this could be part of improper design or RF Pad support welding(fillet)? 

and this question already earlier answered in the group.

this kind of joint can be further welded or joint by weld flange at each and then bolted with insulated bolt., 

however service temperature variation may affect both joint thermal expansion that need to add by metal expansion joint at CS side.

pl do not joint directly by welding. Or else use transition spool as mentioned above if you have multiple WPS's/PQR's to support these welding.