https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/f0bb15a1-0ff5-4d62-b662-1b365472aadbn%40googlegroups.com.
Thanks & Regards
J.Gerald Jayakumar
0091-8838619635
Thanks & Regards
J.Gerald Jayakumar
0091-8838619635
AWS D1.1 does not restrict the number of PQRs supporting a WPS. Clause 6 requires only that essential variables be validated by procedure
qualification testing. Where a single PQR does not cover all required variables of a production WPS, multiple PQRs may be combined to provide
full technical support. Therefore, using multiple PQRs to support one WPS is fully acceptable and code-compliant.
Sridhar.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/716296612.2639809.1772448068895%40mail.yahoo.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAOnS74cq4KK-zTQpm8Bf4F937_mA%2Biy1fSR0nLx7DBG1500NzQ%40mail.gmail.com.
Giving below are the hints for WPS (both ISO / AWS) for joining SS 410 (martensite) to SS 316 (austenitic).
This should be supported by a PQR qualification.
WPS: Dissimilar Joint: SS 410 vs. SS 316
Process: GTAW (Root) + SMAW / GMAW (Fill & Cap); Type: Dissimilar stainless steel welding
SS 410 (UNS S41000) – 410 Martensite SS to SS 316 – Austenitic SS; ASME sec. IX P no 6 (410) to Pno 8 (316)
Joint Type: Butt joint; Thickness Range (Qualified): xx mm – xx mm (based on the PQR)
Root Gap: 2–3 mm; Bevel Angle: 60° included; Backing: Optional (SS backing or GTAW root)
GTAW: ER 309L / ER NiCr-3; SMAW: E 309L / ENiCrFe-3; GMAW: ER309L
(309L acts as a buffer to handle dilution & prevent cracking; Ni-base reduces risk of martensite cracking)
7. PWHT (for SS 410): SR at 650-700 deg C; Holding time- 1hr / 25 mm thick; Cooling- Controlled furnace cooling.
Trust above details will help you to prepare your WPS & PQR.