Dear Team,
   
 I want to confirm about the consumable selection and PWHT requirement (chromium content greater than 3%) for tube to tubesheet joint. Material is listed below,
1. TUBE SHEET:  SA 182 F6A CL2(P#6 Gr.3) 80MM thickness.
2. TUBE : SA 213 T9(P # 5B) 19mm dia 3 mm thickness.
Below confirmation is requested,
1. Consumable for GTAW?
2. PWHT requirement?

Best Regards,
M Bilal

Ch Bilal jovinda

unread,
Nov 5, 2025, 10:53:21 PM (4 days ago) Nov 5
to material...@googlegroups.com
Hi experts, 
   Seeking advice on using ERNiCrMo-3 GTAW wire for welding P No. 6 Gr. 3 to P No. 5B material in a tube-to-tubesheet joint. Any experience or recommendations would be appreciated."
BEST REGARDS,
M Bilal

sridhar cn

unread,
Nov 6, 2025, 5:14:50 AM (4 days ago) Nov 6
to material...@googlegroups.com

 

Mr. Bilal,

Your base metals are, Tube Sheet: SA 182 F6A Cl.2 → P-No. 6, Gr. 3 (13% Cr martensitic stainless steel) 

and Tube: SA 213 T9 → P-No. 5B (9Cr-1Mo ferritic steel).


Recommended GTAW fillers are ER80S-B8 for strength-bearing joints. Though ER309L/ER309LMo are 

used for dissimilar welding between Cr-Mo and martensitic stainless steels, buttering helps prevent hard, 

brittle martensite at the fusion zone. ERNiCr-3 (Inconel 82) is a better choice for providing crack resistance 

and avoiding PWHT; i.e., for buttering, you can use ERNiCr-3, and for tube welding, use ER80S-B8.


PWHT is not required for tube-to-tube sheet seal welds. Buttering with ERNiCr-3 or ER309L also helps to 

avoid  PWHT in the assembly, as it controls hardness.

C Sridhar.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAOq7hqu%3DKuBA5Tc0LRXP2z%3DxCFFv7zob733zCwfjrQm-5JyFHg%40mail.gmail.com.

Ch Bilal jovinda

unread,
Nov 6, 2025, 10:48:18 AM (3 days ago) Nov 6
to material...@googlegroups.com
Dear Sridhar,
   Our joint type is tube to tubesheet and buttering is not accessible. What is your valuable suggession for the selection between ER 80S B9 and ER NiCr-3.