Dear expert,

Any suggestion to prevent centreline crack? i was found centreline crack exist on the first run/layer after backgouging.
base material is S355JR 50mm thick with joint configuration double bevel tee joint full-pen weld by SAW.

Thank you for your help

Rgds,
Gigin

Chirag Sandhane

no leída,
14 jun 2015, 2:30:5314/6/15
a material...@googlegroups.com
Dear gig in,

Cente line crack come in during welding because of following reasons.

1. Your depth to width ratio is high means narrow groove design.
2. There may be high percent of carbon or sulfur or phosphorus in consumable.

Because melting point of sulphur and phosphorus is low, they solidify after sodification of remaining elements.

Thanks & regards.

Gopalakrishnan G

no leída,
14 jun 2015, 2:31:0314/6/15
a material...@googlegroups.com
what s ur joint design? if it is double bevel whether 1/2 on both sides or 2/3 & 1/3 ? preheat temperature?


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/5472638b-731d-405b-b158-0ef2e503b08b%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
G.Gopalakrishnan
Welding Engineer
Mukand Ltd
Mumbai
Moble :+91-9833397917

george....@gr.bureauveritas.com

no leída,
14 jun 2015, 7:15:2114/6/15
a material...@googlegroups.com

did you preheat?
maybe a lot of heat sink and rapid cooling on first pass

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


Inactive hide details for Gopalakrishnan G ---14/06/2015 09:31:10---what s ur joint design? if it is double bevel whether 1/2 oGopalakrishnan G ---14/06/2015 09:31:10---what s ur joint design? if it is double bevel whether 1/2 on both sides or 2/3 & 1/3 ? preheat tempe

.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/CAOp_kKhV2xOVqfzAKmd8ofwYC1PG%3D9FMRR49Y4fsWjUa%3D6%2BUzw%40mail.gmail.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Responder a todos
Responder al autor
Reenviar
0 mensajes nuevos