PWHT of Normalized head

74 views
Skip to first unread message

Muhammed Ibrahim PK

unread,
Apr 14, 2024, 8:56:51 AMApr 14
to material...@googlegroups.com
Gentlemen,

Is PWHT can be avoided if the welded head (2 piece construction) performs normalizing after forming ?

Head MOC : SA516 Gr 70, 45 mm thk, fabricated by welding the blank in two pieces. 

Complete vessel not required PWHT.

Thanks & Regards
Muhammed Ibrahim PK

George Dilintas

unread,
Apr 15, 2024, 12:20:15 AMApr 15
to material...@googlegroups.com
Yes

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALOPgmMorLP3zvhePLHgVGFbcpx-t-%2BSd3M6EQpsfpHrAs38Ow%40mail.gmail.com.

atul jha

unread,
Apr 15, 2024, 4:04:40 AMApr 15
to material...@googlegroups.com
Kindly get a data from design team for fiber elongation if code of construction is divViii and if it is grater then 10 percent PWHT is mandatory.
Regards 
Atul

--

anthony chundal

unread,
Apr 15, 2024, 6:35:05 AMApr 15
to material...@googlegroups.com
Hi

PWHT is required for 45 thk, normalizing is separate heat treatment and cant be combined with stress relieving,

Regards,



--

venkateswara reddy Desireddy

unread,
Apr 15, 2024, 6:35:05 AMApr 15
to material...@googlegroups.com
If dish normalised no need to do PWHT.

G.K.PILLAI

unread,
Apr 15, 2024, 10:53:08 AMApr 15
to material...@googlegroups.com
Normalizing done for head -ok
then how about the weld  of head with shell?

Thanks&Regards,

G.K.PILLAI.

MOBILE

+97433329545    (QATAR)
+919500755882   (INDIA)

--

venkateswara reddy Desireddy

unread,
Apr 15, 2024, 12:59:33 PMApr 15
to material...@googlegroups.com
Hi, 
If you heat treated 900°C , then no need to do 610°C. 

Annamalai Ram

unread,
Apr 16, 2024, 3:18:33 AMApr 16
to Materials & Welding


Normalizing said to heat the steel, above  critical line, A3 and Acm lines and cooling in room temperature (cooling rate normally 500 to 1000°C/hr. For Steel, SA516, Gr70, Carbon is about 0.2% and heated  about to 900°C

PWHT is heating below critical temperature(say around 650°C) and heating and holding and cooling rate are controlled(often below 100°C/hr).

For pressure vessel purpose, ASME Sec VIII, Div1, Table UCS-56.1 is normally followed.  For thickness, 45mm, Div2 is suggested. Heating and cooling rates are normally followed per ANSI B31.1, Table.132. 

Most of the pressure welds, requiring PWHT, are Procedure Qualified, including PWHT.

So, Normalizing and PWHT are not comparable. We need more data like hardness, grain size etc after heat treatment.

Muhammed Ibrahim PK

unread,
Apr 16, 2024, 3:18:33 AMApr 16
to material...@googlegroups.com
PWHT required specific holding time and controlled cooling as per sec VIII Div.1. Normalizing having air cooling after reaching at 900 deg c.  Since normalizing not required specified holding time and controlled cooling, will it substitute ?


Thanks & Regards
Muhammed Ibrahim PK

Prakash Hegde

unread,
Apr 16, 2024, 4:32:59 AMApr 16
to material...@googlegroups.com, Muhammed Ibrahim PK
Hi
Generally CS sa516 plates supplied in.NR condition i.e heating to above Ac3 about 900c and cooled in still air

As per ASME code Welded vessel above above 38mm nominal thk.req PWHT below Ac1as per UCS56 of course for sour /lethal service all the Vessels req PWHT irrespective of.nominal thk.

Regards
Hegde Prakash


On Tue, 16 Apr 2024 at 12:48, Muhammed Ibrahim PK

Vishwas Keskar

unread,
Apr 16, 2024, 10:11:42 PMApr 16
to material...@googlegroups.com, Muhammed Ibrahim PK
As I understand it  correctly ,
there are two joints  in Head.
So need PQR to be qualified with Normalising .
Ensure consumable strength  withstands this Normalising .
Div 1 is lenient about the Normalising HT of the Weld and Head.
Mfg has to establish the procedure thr SOP and need Test coupon as a simulation Fabrication Test coupon.
Attach the FTC as an extension on Head and test it . Shall comply to SA 516 Gr 70 
Only Normalising would have been suffice but there are joints . so pl follow PWHT as per UCS 56 Table 1 after Normalising .
Let head shall undergo PWHT separate if your Vessel is exempted of PWHT due to Design
Vishwas
IWE - International Welding Engineer

Sent from my iPhone