1018 is an AISI designation that specifies chemistry only although standards other than the general ASTM/SA-A29 might specify. AISI 1018 is a carbon steel with a nominal carbon content of 0.18%.
For example:
A/SA-311 Specification for cold-drawn, stress-relieved carbon steel bars subject to mechanical property requirements
Varies on diameter/thickness
|
Thickness/diameter in. (mm) |
Tensile ksi (MPa) |
Yield ksi (MPa) |
Elongation - RA |
|
< 7/8 (20) |
70 (480) |
60 (415) |
18 - 40 |
|
>7/8 (20) to < 1¼ (30) |
65 (450) |
55 (380) |
16 - 40 |
|
>1¼ (30) to < 2 (50) |
60 (415) |
50 (345) |
15 - 35 |
|
>2 (50) to < 3 (75) |
55 (380) |
45 (310) |
15 - 35 |
|
|
|
|
|
You might also look at other specifications referenced in A/SA-29.
Hope this helps. Code is fun. “Live long and prosper” (Mr. Spock)
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-weld...@googlegroups.com.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/a7066f2f-0075-4d37-9c9c-f28526554fcc%40googlegroups.com.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/a7066f2f-0075-4d37-9c9c-f28526554fcc%40googlegroups.com.
Ing. José Juan Jiménez Alejandro
Independent Consultant in Parts
and Pressure Equipment
SSI-TPI
Móvil +52 1 812 352 4606
Skype: jjjimeneza
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/a7066f2f-0075-4d37-9c9c-f28526554fcc%40googlegroups.com.