Dear Sir,
I come across critical situation of welding with cast iron to carbon steel plate.cast iron Material IS2707 GR1 to SA 516 GR 70 or SA 36 (plate).

Following chemical composition of cast iron:
Carbon: 0.472%,Mn: 0.891%,Si: 0.566%,P: 0.04%,S:0.04%

  Kindly suggest us SMAW welding electrodes and preheat and post heating requirement during welding of same dissimilar base metal.

Regards,
Vivek Pandey

prem_nautiyal26

unread,
Oct 25, 2016, 10:46:22 PM10/25/16
to material...@googlegroups.com, pgoswami
Hi

If Carbon content is more than 1.6% they are called cast irons.

In your case it is a high carbon steel. 

Regards

Prem Nautiyal 
9769316004




Sent from my Samsung Galaxy smartphone.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANCwoYnG1zC_osifwAB%2BSS_O5r%3DMjN1s8Fj%3DHLeVT7Wvti%3Dngg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

SHANMUGA PERUMAL

unread,
Oct 25, 2016, 11:53:52 PM10/25/16
to material...@googlegroups.com

Refer IS 5530.
Regards,
Shanmuga perumal.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

Kannayeram Gnanapandithan

unread,
Oct 26, 2016, 12:11:27 AM10/26/16
to materials-welding
It is not Cast Iron, It is Carbon Steel casting with high carbon. U can use E7018-1 with preheat and post heating

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,