Dear expertsWe have job with MDMT -30 and -36 Deg CShell/Dish - SA516 Gr 70Nmaterial will be received in impact tested conditionneed to know whether weld impact test is required or not?thickness is 8-10 mm.welding electrode 7018-1Thanksprateik
I presume there is no specific service requirements based impact testing and plates are normalized
As per Figure UCS-66M of ASME Sec 8 Div.1, The material 516 fouls under curve D. the impact testing is exempted up to -48°C for your thickness. So not required for your case.
Thanks and Regards
Rameshkannan Devaraj
"What you have learned is a mere handful; What you haven't learned is
the size of the world – Avvaiyar"
Dear expertsWe have job with MDMT -30 and -36 Deg CShell/Dish - SA516 Gr 70Nmaterial will be received in impact tested conditionneed to know whether weld impact test is required or not?thickness is 8-10 mm.welding electrode 7018-1On Wed, Feb 19, 2020 at 2:06 PM prateik tolani <tolani...@gmail.com> wrote:Dear expertsWe have job with MDMT -30 and -36 Deg CShell/Dish - SA516 Gr 70Nmaterial will be received in impact tested conditionneed to know whether weld impact test is required or not?thickness is 8-10 mm.welding electrode 7018-1Thanksprateik
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAGNY-_AMkqLQr%2BV0KXTtf%3DG%2BX03SpPg8z92ePJqHXO0PJpZctg%40mail.gmail.com.
I presume there is no specific service requirements and plates are normalized
As per Figure UCS-66M of Sec 8 Div.1, The plate material 516 fouls under curve D. the impact testing is exempted up to -48°C .
Reg welding, The electrode E7018-1 is guaranteed impact values at -45°C. Refer Table 3 of SFA 5.1.
But its better to have impact tested PQRs for company future use.
Thanks and Regards
Rameshkannan Devaraj
"What you have learned is a mere handful; What you haven't learned is
the size of the world – Avvaiyar"
Dear expertsWe have job with MDMT -30 and -36 Deg CShell/Dish - SA516 Gr 70Nmaterial will be received in impact tested conditionneed to know whether weld impact test is required or not?thickness is 8-10 mm.welding electrode 7018-1On Wed, Feb 19, 2020 at 2:06 PM prateik tolani <tolani...@gmail.com> wrote:Dear expertsWe have job with MDMT -30 and -36 Deg CShell/Dish - SA516 Gr 70Nmaterial will be received in impact tested conditionneed to know whether weld impact test is required or not?thickness is 8-10 mm.welding electrode 7018-1Thanksprateik
--
Dear expertsWe have job with MDMT -30 and -36 Deg CShell/Dish - SA516 Gr 70Nmaterial will be received in impact tested conditionneed to know whether weld impact test is required or not?thickness is 8-10 mm.welding electrode 7018-1On Wed, Feb 19, 2020 at 2:06 PM prateik tolani <tolani...@gmail.com> wrote:Dear expertsWe have job with MDMT -30 and -36 Deg CShell/Dish - SA516 Gr 70Nmaterial will be received in impact tested conditionneed to know whether weld impact test is required or not?thickness is 8-10 mm.welding electrode 7018-1Thanksprateik
--
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMaSVcHs5XyOXpGeyN2r%2B%3D2C6Yej%2BWoRt2AucX%2Bjh_6xN4eTew%40mail.gmail.com.
Dear expertsWe have job with MDMT -30 and -36 Deg CShell/Dish - SA516 Gr 70Nmaterial will be received in impact tested conditionneed to know whether weld impact test is required or not?thickness is 8-10 mm.welding electrode 7018-1On Wed, Feb 19, 2020 at 2:06 PM prateik tolani <tolani...@gmail.com> wrote:Dear expertsWe have job with MDMT -30 and -36 Deg CShell/Dish - SA516 Gr 70Nmaterial will be received in impact tested conditionneed to know whether weld impact test is required or not?thickness is 8-10 mm.welding electrode 7018-1Thanksprateik
--
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMaSVcHs5XyOXpGeyN2r%2B%3D2C6Yej%2BWoRt2AucX%2Bjh_6xN4eTew%40mail.gmail.com.
Thanks and Regards
Rameshkannan Devaraj
"What you have learned is a mere handful; What you haven't learned is
the size of the world – Avvaiyar"
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eOxFw8YR6iF1yOFoBR%2BHiwSdUL39SFU7%2Bo6pm8mt0jqZw%40mail.gmail.com.

Thanks and Regards
Rameshkannan Devaraj
"What you have learned is a mere handful; What you haven't learned is
the size of the world – Avvaiyar"
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAAkMc%3D6GaD_gJ7K9S%2Bt9%3DjDqCmyyeS1s9WxRWB6%3DZ2WDf4%2B4Fg%40mail.gmail.com.