Dear Metallurgists ,

Could you please explain that,

why lateral expansion value of Min. 0.38 mm given in ASME Sec VIII Div I , UHA-51 for Charpy Impact Tests, instead of Joule Value for High Alloy steels like Duplex, Super Duplex etc.

What is the significance of Lateral expansion for such High Alloys.

Regards,
Saravanan.

pgoswami

oläst,
6 jan. 2015 08:25:232015-01-06
till material...@googlegroups.com
Saravanan,
 
Lateral expansion is a measure of ductility in addition to absorbed impact energy(impact values). Austenitic alloys always fail in ductile mode , with very high impact strength. Higher the ductility more is the LE. As these alloys have an inherent ductile nature , causing high impact values, the other way screen them is though lateral expansion.
 
Please see the links below and also ASTM/ASME -A/SA-370.
 
Thanks
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Saravanan Sornam
Sent: Tuesday, January 06, 2015 2:58 AM
To: material...@googlegroups.com
Subject: [MW:22679] Lateral Expansion - High Alloy Impact test

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALV1rkKr_DRJNkPC5H-5Wwj16i0KubE370PKEXtxOrgbdUFBTw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

meisam shokri arfaei

oläst,
6 jan. 2015 10:32:072015-01-06
till material...@googlegroups.com
Some alloy steels shown better relationship between actual impact properties with lateral expansion instead of joules value of absorbed energy. This has been practiced in papers specially in case of high absorbed energies.

Regards

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALV1rkKr_DRJNkPC5H-5Wwj16i0KubE370PKEXtxOrgbdUFBTw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer





Saravanan Sornam

oläst,
7 jan. 2015 02:31:212015-01-07
till material...@googlegroups.com
Dear Pradip Ji,

Thank you for your reply .

Being new to the company, when I review the previously tested PQR on 2012 for Duplex UNS 31803 , i have found the following issues :

1) Only Joule value issued for Charpy Impact Test , tested at -51 Deg C and all the values are more than 100 J , but Lateral Expansion value is not mentioned in test report.
    Can we still accept this Test report as per ASME Sec VIII Div I, UHA 51 to use for ASME jobs?

2) In Chemical Analysis, the obtained Nickel is 7.12%, but as per ASME Part II C, SFA 5.9, ER2209, the range is 7.5 to 9.5 %, 
    I am sure this is not acceptable, isn't it ? 

    Ferrite Analysis is Min. 40% obtained, Micro, Macro , Pttting Corrosion as per G48 method A and other test results are acceptable as per ASME-IX requirements.

But unfortunately, the above 2 issues were overlooked by the former QC and well renowned TPI in Korea, they signed WPS & PQR alongwith this report.