Consumable selection

52 views
Skip to first unread message

Mustaq Ahmad

unread,
Jul 20, 2016, 9:35:58 AM7/20/16
to Materials & Welding
Dear experts

I have ltcs material A333GR6 how to select the consumables for this material please tell me as I am not really aware

Mohit Aggarwal

unread,
Jul 20, 2016, 11:57:35 AM7/20/16
to materials-welding

Hello Mr. Mustaq,

You will have to also mention the service temperature and other requirements..

Generally for SA333GR 6 consumable used is E7018-1, ER 70-S2 which can give Impact properties upto minus 45 deg C with PWHT and Non PWHT also.

Best Regards,
Mohit Aggarwal.
CSWIP 3.1
Sr. Engineer-Welding.

On Jul 20, 2016 7:05 PM, "Mustaq Ahmad" <must...@gmail.com> wrote:
Dear experts

I have ltcs material A333GR6 how to select the consumables for this material please tell me as I am not really aware

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/dc1e199c-d241-488f-876b-73353c77568d%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

José Juan Jiménez Alejandro

unread,
Jul 20, 2016, 11:58:51 AM7/20/16
to material...@googlegroups.com

Filler Metal ASME is ER80SD2. Material SA333 GR 6 to chlorine pipeline.

El 20/07/2016 08:35, "Mustaq Ahmad" <must...@gmail.com> escribió:
Dear experts

I have ltcs material A333GR6 how to select the consumables for this material please tell me as I am not really aware