Dear Experts,

We have done PMION weld joint of INCONEL625 i.e. ENiCrMo-3
Found
Ni -61, Cr-24.6, 25.6, Mo-8.5, Nb -3.37,

Now, As per procedure & code i. e.
Sec II C Cr range is 20-23 given
all other elements are in range.
And PMI analyzer also display Inconel 625.
Please confirm whether it is acceptable or not i.e. chromium %

Best Regards,
Mohit Aggarwal.

pradip kumar Sil

unread,
Feb 12, 2015, 11:11:49 PM2/12/15
to materials-welding
Follow PFS standard, 10% bilateral tolerance on parent material & 12.5 % tolerance  on weld material. 
Chk composition on ASME SEC II

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALTezPOtBHVu5HvuVxdG24WR3uCSsH5sXQkAGkf7C1eLug-r0A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Saravanan Sornam

unread,
Feb 13, 2015, 12:55:17 AM2/13/15
to material...@googlegroups.com
Dear Experts,

based on the below conversation, 

incase a fabricator owns a PMI machine,

what will be the Tolerance for chemical elements ( base metal and Weld metal )  and what is the accuracy level for calibrating the PMI machine.

Regards,
Saravanan

Jignesh Desai

unread,
Feb 13, 2015, 3:04:46 AM2/13/15
to material...@googlegroups.com
For the tolerance on obtained element analysis below standards with relevant para may be referred to resolve the issue.

1. ASME Sec I - Appendix B, para B8.2  (± 10% of standard figure)
2. ASTM A 751 (Tolerance on product analysis) 
3. PFI ES 24 (Para 9.3.1 & 9.3.2).- (± 10 for Base metal & ±12.5 for weld metal)

Regds/Jignesh

On Friday, 13 February 2015 09:41:49 UTC+5:30, pradipsil wrote:
Follow PFS standard, 10% bilateral tolerance on parent material & 12.5 % tolerance  on weld material. 
Chk composition on ASME SEC II
On Fri, Feb 13, 2015 at 5:12 AM, Mohit Aggarwal <aggarwa...@gmail.com> wrote:

Dear Experts,

We have done PMION weld joint of INCONEL625 i.e. ENiCrMo-3
Found
Ni -61, Cr-24.6, 25.6, Mo-8.5, Nb -3.37,

Now, As per procedure & code i. e.
Sec II C Cr range is 20-23 given
all other elements are in range.
And PMI analyzer also display Inconel 625.
Please confirm whether it is acceptable or not i.e. chromium %

Best Regards,
Mohit Aggarwal.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

Mohan Kumar

unread,
Feb 13, 2015, 10:52:46 AM2/13/15
to material...@googlegroups.com
PMI results should be considered only for validation and not as acceptance. If any doubt in chemical composition grind off few sample and send it to lab for chemical analysis.

Regards 
Mohan

For more options, visit https://groups.google.com/d/optout.


--
Regards
Mohankumar

Mohit Aggarwal

unread,
Feb 13, 2015, 11:09:45 PM2/13/15
to materials-welding

Dear Sir,
I have Checked ASME Sec.IIC after that only I have queried about.

Please let me know about bilateral tolerance for weld,where it is given in SecIIC

Best Regards,
Mohit Aggarwal.