Regarding Welder Qualification

63 views
Skip to first unread message

Mohit Aggarwal

unread,
Mar 20, 2017, 1:16:29 PM3/20/17
to materials-welding
Dear Experts,

As per ASME Sec IX if for small diameter we have to done qualification e.g. 1/2" dia . Pipe we will have to take multiple specimen to cover the 150 mm length for RT, and also we Can't take specimen more than 4 nos.

I have query which dia we will have to consider for qualification of welder it's Outer dia. Or Inner dia of pipe for circumference length calculation because if we will consider inner dia for calculation then we will have to take more than 4 specimens and which violates the code .

Best Regards,
Mohit Aggarwal

dilintas

unread,
Mar 22, 2017, 10:37:21 PM3/22/17
to material...@googlegroups.com
Outside diameter 



Sent from my Samsung Galaxy smartphone.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALTezPOruStAVdWvREdMUJv4RZQRguYF_9nhW2HM%3DozBKeRhsA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Mohit Aggarwal

unread,
Mar 23, 2017, 2:32:07 AM3/23/17
to materials-welding
Dear Sir,

Kindly confirm the reference but when we done the root welding this is towards ID and how OD can be considered for calculation?

Regards,
Mohit Aggarwal

On Mar 23, 2017 8:07 AM, "dilintas" <dili...@gmail.com> wrote:
Outside diameter 



Sent from my Samsung Galaxy smartphone.

-------- Original message --------
From: Mohit Aggarwal <aggarwa...@gmail.com>
Date: 20/03/2017 10:12 (GMT+02:00)
To: materials-welding <materials-welding@googlegroups.com>
Subject: [MW:26234] Regarding Welder Qualification

Dear Experts,

As per ASME Sec IX if for small diameter we have to done qualification e.g. 1/2" dia . Pipe we will have to take multiple specimen to cover the 150 mm length for RT, and also we Can't take specimen more than 4 nos.

I have query which dia we will have to consider for qualification of welder it's Outer dia. Or Inner dia of pipe for circumference length calculation because if we will consider inner dia for calculation then we will have to take more than 4 specimens and which violates the code .

Best Regards,
Mohit Aggarwal

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/o7q0f8y2ty7cccds7n68lntf.1490203043482%40email.android.com.

Kannayeram Gnanapandithan

unread,
Mar 23, 2017, 6:13:31 AM3/23/17
to materials-welding
Ref Table QW 452.4. As Dilinta said, it is only OD

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Thu, Mar 23, 2017 at 11:59 AM, Mohit Aggarwal <aggarwa...@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (aggarwa...@gmail.com) Add cleanup rule | More info

Dear Sir,

Kindly confirm the reference but when we done the root welding this is towards ID and how OD can be considered for calculation?

Regards,
Mohit Aggarwal
On Mar 23, 2017 8:07 AM, "dilintas" <dili...@gmail.com> wrote:
Outside diameter 



Sent from my Samsung Galaxy smartphone.

-------- Original message --------
From: Mohit Aggarwal <aggarwa...@gmail.com>
Date: 20/03/2017 10:12 (GMT+02:00)
To: materials-welding <materials-welding@googlegroups.com>
Subject: [MW:26234] Regarding Welder Qualification

Dear Experts,

As per ASME Sec IX if for small diameter we have to done qualification e.g. 1/2" dia . Pipe we will have to take multiple specimen to cover the 150 mm length for RT, and also we Can't take specimen more than 4 nos.

I have query which dia we will have to consider for qualification of welder it's Outer dia. Or Inner dia of pipe for circumference length calculation because if we will consider inner dia for calculation then we will have to take more than 4 specimens and which violates the code .

Best Regards,
Mohit Aggarwal

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/o7q0f8y2ty7cccds7n68lntf.1490203043482%40email.android.com.

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALTezPMpNysTAGXq2CeB%3D68ybeB2dtq1YwvYT4TCuw_K5hMADQ%40mail.gmail.com.

dilintas

unread,
Mar 24, 2017, 12:31:38 AM3/24/17
to material...@googlegroups.com
Always the OD




Sent from my Samsung Galaxy smartphone.

-------- Original message --------
From: Mohit Aggarwal <aggarwa...@gmail.com>
Date: 23/03/2017 08:29 (GMT+02:00)
To: materials-welding <material...@googlegroups.com>
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

MESAB Engineering & Contracting Co

unread,
Mar 24, 2017, 7:39:09 AM3/24/17
to material...@googlegroups.com
Dear sir 

the RT film should min 150 mm length 
must calculation from out side the pipe wall , 
confirm to Mr Dainilta said .

Best Regards 
Saad Olimat 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

Raju Kandula

unread,
Mar 24, 2017, 10:38:22 PM3/24/17
to material...@googlegroups.com
ASME SEC IX QW302.2

the minimum length of coupon(s) to be examined
shall be 6 in. (150 mm) and shall include the entire weld
circumference for pipe(s), except that for small diameter
pipe, multiple coupons may be required, but the number
need not exceed four consecutively made test coupons

Reply all
Reply to author
Forward
0 new messages