Suitability of PWHT on ER309L Buttering over CS

281 views
Skip to first unread message

kunalen...@gmail.com

unread,
Jul 22, 2020, 8:04:50 AM7/22/20
to Materials & Welding
Dear Experts

Need your expert advice that we have a joint of CS to SS, PWHT is applicable for CS. So planned to go for the buttering with ER309L & then PWHT prior welding with SS. Please advise does ER309L has any adverse effect on it if comes under the PWHT cycle applicable for P1 material.

Kannayeram Gnanapandithan

unread,
Jul 22, 2020, 9:42:26 AM7/22/20
to materials-welding
309 weld metal may not be suitable for temperature above 370°C. Due to sigmaphase formation

On Wed, 22 Jul 2020 5:34 pm , <kunalen...@gmail.com> wrote:
Dear Experts

Need your expert advice that we have a joint of CS to SS, PWHT is applicable for CS. So planned to go for the buttering with ER309L & then PWHT prior welding with SS. Please advise does ER309L has any adverse effect on it if comes under the PWHT cycle applicable for P1 material.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/06110dfb-3346-4a70-bc6c-01f5fcf47d69o%40googlegroups.com.

TDK YOKESH

unread,
Jul 22, 2020, 12:04:07 PM7/22/20
to material...@googlegroups.com
You can use Inconel filler for buttering to avoid intermetallic phase formation during pwht. 

On Wed, Jul 22, 2020, 4:04 PM <kunalen...@gmail.com> wrote:
Dear Experts

Need your expert advice that we have a joint of CS to SS, PWHT is applicable for CS. So planned to go for the buttering with ER309L & then PWHT prior welding with SS. Please advise does ER309L has any adverse effect on it if comes under the PWHT cycle applicable for P1 material.

--

pgos...@rogers.com

unread,
Jul 22, 2020, 5:04:23 PM7/22/20
to material...@googlegroups.com, kunalen...@gmail.com

Hi Kunalenfield,

 

You may use 309L for buttering on carbon steel and subsequent PWHT, provided the design conditions do not exceed the recommendations of API RP-582 as below. A buttering PQR should be established according to ASME Sec-IX , QW -283 . Typical buttering thickness to lesson the effects of welding on the buttered surface should be 3/16”. Read the details of QW-283 to establish a buttering followed by welding on the same test coupon.

 

Thanks.

 

 

P.Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

 

--

https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/06110dfb-3346-4a70-bc6c-01f5fcf47d69o%40googlegroups.com.


Virus-free. www.avg.com
image002.png

erojas

unread,
Jul 22, 2020, 11:02:31 PM7/22/20
to Materials & Welding
 The nickel-base alloy filler metals