I am wondering if anyone knows what the maximum weave is for SMAW (specifically ASME Section VIII Div 1). For some reason 3x is sticking in my brain, but I would like to know where to find it in the ASME Codes.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/24ee9b7d-4956-4f4d-8a40-86b41259ea8f%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
I am wondering if anyone knows what the maximum weave is for SMAW (specifically ASME Section VIII Div 1). For some reason 3x is sticking in my brain, but I would like to know where to find it in the ASME Codes.
--
I am wondering if anyone knows what the maximum weave is for SMAW (specifically ASME Section VIII Div 1). For some reason 3x is sticking in my brain, but I would like to know where to find it in the ASME Codes.
--
Incorrect information.
First PW-40 is in Section I not Section VIII, so does not apply top question asked.
Second, PW-40.3.4 (d), which references bead width, applies only to repairs performed by the temper bead or half bead technique. Very specialized application.
Third, there is no restriction otherwise on bead width in either Section VIII, Division 1, or Section I.
One will often find such restrictions in customer specifications.
Careful where you walk. Free advice is worth just that.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4ePbq-NLnjvGkA_Ee34FUEAXPQWJcSFrk_VCHBsWd0VR8Q%40mail.gmail.com.
Again, incorrect information.
Section VIII, UCS-56.f.4(-a) applies only to repairs avoiding PWHT by use of temper bead or half bead technique. See UCS-56.f.4(-c).
There is no weave width restriction for general welding in either Section VIII, Div. 1, or Section I.
Do not apply special case requirements to general welding. A recurring mistake made by many.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/32C2F815-0F38-4873-A911-0E5C70994009%40gmail.com.
| From: John Henning Sent: Δευτέρα, 23 Μαΐου 2016 - 18:11 Reply To: material...@googlegroups.com Subject: RE: [MW:24835] Weare or string |