Welding Parameter for HP modification (25Cr-35Ni-0.1C+Nb) Material

86 views
Skip to first unread message

tuan...@gmail.com

unread,
Jan 14, 2020, 3:51:58 AM1/14/20
to Materials & Welding
Dear Experts 
Please suggest a good welding parameter for HP modification (25Cr-35Ni-0.1C+Nb) Material 
Welding consumable, PWHT if need.

Thank you 

N.A. Tuan


Karthik

unread,
Jan 14, 2020, 4:09:41 AM1/14/20
to Materials & Welding
Hi,
Go with ENiCrFe-2 (Incoweld A) or ENiCrCoMo3 (Inconel 617). No PWHT needed. You may preheat up to maximum of 75 degree Celsius.

Thanks& Regards,

 

(Karthik)

Karthikeyan.S

E-mail : karthi...@yahoo.com



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/525e8e0a-6c8b-4f00-bc35-f83b20bbb085%40googlegroups.com.

Kannayeram Gnanapandithan

unread,
Jan 14, 2020, 6:58:58 AM1/14/20
to materials-welding
Any interpass temperature restrictions

Dinesh Somwanshi

unread,
Jan 14, 2020, 6:59:03 AM1/14/20
to materials-welding
Dear sir,

Incoloy 617,   Need to maintain underpass strictly to 125 degrees.

PWHT may need if your service temperature exceeds 550 deg centigrade.

regards

Dinesh


Karthik

unread,
Jan 14, 2020, 8:04:52 AM1/14/20
to material...@googlegroups.com
Nice question. Yes, interpass temperature should be controlled to maximum of 250 degree Celsius.


Sent from Yahoo Mail for iPhone