Dear Experts,

Please give me the guide for Hard facing Overlay:
We did a) Visual Examination, b) LPT, c) Hardness Test, d) Macro, e)
Weld Metal chemical analysis.
Is there any other mechanical or other test required for HFO like
Tensile or Bend test required?
Please guide me with ASME Sec IX 2010.

--
Thanks & Regards
Biplab Pal
Welding Inspector
E-mail: bipla...@gmail.com

Information in this email and any attachments is confidential and intended
solely for the use of the individual(s) to whom it is addressed or
otherwise directed. Please note that any views or opinions presented in
this email are solely those of the author and do not necessarily represent
those of the Company. Finally, the recipient should check this email and
any attachments for the presence of viruses. Myself accepts no liability
for any damage caused by any virus transmitted by this email.

james gerald

unread,
May 23, 2013, 12:43:45 AM5/23/13
to material...@googlegroups.com
Refer QW-453.
 
I suppose there is no other requirement as mentioned in your mail.
 
Thanks & Regards

J.Gerald Jayakumar
00968-99438165
From: Biplab Pal <bipla...@googlemail.com>
To: materials-welding <material...@googlegroups.com>; Chandan Majumdar <majum...@yahoo.co.in>; chandan.majumdar <chandan....@sgs.com>
Sent: Thursday, May 23, 2013 12:33 AM
Subject: [MW:17743] Hard Facing Overlay Test Required
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.




zakir ali

unread,
May 23, 2013, 2:25:00 AM5/23/13
to material...@googlegroups.com
Dear Pal,

Chemical test is not mandatory for HFO.
There is no other tests apart from what U have mentioned.


Regards,

Zakir Ali.



From: james gerald <gerr...@yahoo.com>
Sent: Thu, 23 May 2013 11:47:29
To: "material...@googlegroups.com" <material...@googlegroups.com>
Subject: Re: [MW:17756] Hard Facing Overlay Test Required
Refer QW-453.
 
I suppose there is no other requirement as mentioned in your mail.

Thanks & Regards

J.Gerald Jayakumar
00968-99438165
From: Biplab Pal <bipla...@googlemail.com>
To: materials-welding <material...@googlegroups.com>; Chandan Majumdar <majum...@yahoo.co.in>; chandan.majumdar <chandan....@sgs.com>
Sent: Thursday, May 23, 2013 12:33 AM
Subject: [MW:17743] Hard Facing Overlay Test Required

Dear Experts,

Please give me the guide for Hard facing Overlay:
We did a) Visual Examination, b) LPT, c) Hardness Test, d) Macro, e)
Weld Metal chemical analysis.
Is there any other mechanical or other test required for HFO like
Tensile or Bend test required?
Please guide me with ASME Sec IX 2010.

--
Thanks & Regards
Biplab Pal
Welding Inspector


Information in this email and any attachments is confidential and intended
solely for the use of the individual(s) to whom it is addressed or
otherwise directed. Please note that any views or opinions presented in
this email are solely those of the author and do not necessarily represent
those of the Company. Finally, the recipient should check this email and
any attachments for the presence of viruses. Myself accepts no liability
for any damage caused by any virus transmitted by this email.

--
To post to this group, send email to material...@googlegroups.com" >material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com" >unsub...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com." >unsub...@googlegroups.com.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

For more options, visit https://groups.google.com/groups/opt_out.
 
 


Get your own FREE website and domain with business email solutions, click here

prem nautiyal

unread,
May 23, 2013, 10:30:59 AM5/23/13
to material...@googlegroups.com, Chandan Majumdar, chandan.majumdar
Hi
Assuming that you are running a PQR, As per ASME Sec IX , QW-453 following test are required for procedure qualification of HFO:
(3) The hard-facing surface shall be examined by the liquid penetrant method and shall meet the acceptance standards in QW-195.2 or as specified
in the WPS. Surface conditioning prior to liquid penetrant examination is permitted.
(7) After surface conditioning to the minimum thickness specified in the WPS, a minimum of three hardness readings shall be made on each of
the specimens from the locations shown in QW-462.5(b) or QW-462.5(e). All readings shall meet the requirements of the WPS.
(8) The base metal shall be sectioned transversely to the direction of the hard-facing overlay. The two faces of the hard-facing exposed by sectioning
shall be polished and etched with a suitable etchant and shall be visually examined with 5 magnification for cracks in the base metal or the
heat-affected zone, lack of fusion, or other linear defects. The overlay and the base metal shall meet the requirements specified in the WPS.
All exposed faces shall be examined. See QW-462.5(b) for pipe and QW-462.5(e) for plate.
(9) When a chemical composition is specified in the WPS, chemical analysis specimens shall be removed at locations specified in QW-462.5(b)
or QW-462.5(e). The chemical analysis shall be performed in accordance with QW-462.5(a) and shall be within the range specified in the
WPS. This chemical analysis is not required when a chemical composition is not specified on the WPS.
 
 
You have covered all the tests as per QW-453.
Regards
Prem Nautiyal

 
From: Biplab Pal <bipla...@googlemail.com>
To: materials-welding <material...@googlegroups.com>; Chandan Majumdar <majum...@yahoo.co.in>; chandan.majumdar <chandan....@sgs.com>
Sent: Thursday, May 23, 2013 2:03 AM
Subject: [MW:17743] Hard Facing Overlay Test Required
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsub...@googlegroups.com.

sathish

unread,
Dec 15, 2019, 10:09:49 PM12/15/19
to Materials & Welding
Dear Expert
As i have weld deposit to 4-5mm ERCoCr-A on Astm A36 and 1.6mm finished thick of weld metal from base metal.
1. on 1.6mm I have made chemical analysis, my doubt is that did i need to verify the element of chemical avilable for ERCoCr-A filler wire from ASME Sec II Part-C.

If i check Fe value is not meeting to Filler wire, As the Base metal having Fe about >98% and filler wire 3% on dilution and taking test at 1.6mm it is not achievable.

Kindly suggest some inputs on this requirement


Regards
S.Sathish kumar 

raghul k

unread,
Dec 16, 2019, 12:56:50 AM12/16/19
to material...@googlegroups.com
Dear sathish,

              On overlay.chemical analysis will be related to PREN (Pitting resistance equivalent number) not to asme sec II part C.


---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/483f1f8d-925d-4436-8f09-5eb3dc2a363c%40googlegroups.com.

sathish

unread,
Dec 16, 2019, 6:13:45 AM12/16/19
to Materials & Welding
Dear Mr.Ragul
Thanks for the response.

How to ensure that PREN meeting the chemical analysis. I have tested Welding of ERCoCr-A PTAW powder with ASTM A36, SS316L, F11,F22,F91 MATERIALS.

 Can you provide which standard or value to refer for acceptance and how to check the same?


Regards
S.Sathish kumar

On Thursday, 23 May 2013 02:03:26 UTC+5:30, Biplab Pal wrote:

raghul k

unread,
Dec 16, 2019, 10:24:38 PM12/16/19
to material...@googlegroups.com
HI,
        Actually when i worked in Aramco project,They recommended min PREN value for overlay portion as per SAES.

common formula for PREN value=%cr+3.3 X Mo%+16 x N%

           

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

Kannayeram Gnanapandithan

unread,
Dec 16, 2019, 11:59:01 PM12/16/19
to materials-welding
What you have welded is not a Corrosion Resistance overlap, it is a Hardsurfacing overlap, in which no PRN required. Only Hardness value is required. Thanks

sathish

unread,
Dec 17, 2019, 5:07:36 AM12/17/19
to Materials & Welding
Dear Sir
But in QW-453, Note:9 mentioned for chemical composition for hardfacing overlay procedure qualification testing?


On Thursday, 23 May 2013 02:03:26 UTC+5:30, Biplab Pal wrote:

Kannayeram Gnanapandithan

unread,
Dec 19, 2019, 2:36:27 AM12/19/19
to materials-welding
Ref QW 216, QW 453 and QW 462.5(a)
you will be clear about requirements. 
Unless specified/requirement, u need do chemical analysis for Hard surfacing Overlay. 
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Reply all
Reply to author
Forward
0 new messages