Kindly advice

in general major clients write in thier specs FCAW process not allowed in presure vessel & pressure pining joints

Ramesh

unread,
Feb 12, 2020, 1:00:30 AM2/12/20
to material...@googlegroups.com
The FCAW restrictions  as below 


 

The FCAW Gas Shielded process shall not be used for the root pass on full penetration, groove joints that are welded from one side only without backing

 

The FCAW   self-shielded shall only be permitted prior approval through pWPS with full matrix of proposed testing



Thanks and Regards


Rameshkannan Devaraj

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"



On Wed, Feb 12, 2020 at 9:23 AM Chintan <chin...@gmail.com> wrote:
Kindly advice

in general major clients write in thier specs FCAW process not allowed in presure vessel & pressure pining joints

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/926b0970-558d-47f7-8c53-3de21d008787%40googlegroups.com.

SENTHILKUMAR SWAMINATHAN

unread,
Feb 12, 2020, 2:14:12 AM2/12/20
to material...@googlegroups.com
It'scorrect I have experienced Root LOF found all the way. Bcoz of high weld metal deposition rate Double V ideal case or Back gouging is required. 
Regards, 

Kannayeram Gnanapandithan

unread,
Feb 12, 2020, 2:14:12 AM2/12/20
to materials-welding
No Restriction in using FCAW. Ref ASME SEC 8, Div 1, UW-27-Welding process

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


Reply all
Reply to author
Forward
0 new messages