We have a job with 30 degree single bevel corner joint, as per client requirement we are using SAW process to complete on time schedule.
the fact is for root run the slag is not easy to be removed, as its hard and taking a lot of time even for grinding wheel / chipping. can some one say the reason for it. or a solution. 
Subsequent layers  slag is releasing on it's own, so i don't doubt filler metal or flux.
we are at present using base metal 20mm thk and 4mm filler metal, brand, D&H.

Regards,
Dharma Dattu. B

Kannayeram Gnanapandithan

unread,
Dec 16, 2019, 12:56:50 AM12/16/19
to materials-welding
This is due to joint design, deeper / narrow the joint difficult to remove slag

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/ff2af474-4f1c-48e0-8ee6-e284a0228a4e%40googlegroups.com.

Dharma dattu

unread,
Dec 16, 2019, 4:43:31 AM12/16/19
to Materials & Welding
Sir,
I is there any solution as for welding it takes 1 hour, for clearing slag it's taking more than 3 hours.

Regards,

Dharma Dattu. B


On Monday, 16 December 2019 11:26:50 UTC+5:30, kannayeram gnanapandithan wrote:
This is due to joint design, deeper / narrow the joint difficult to remove slag

On Mon, 16 Dec 2019 8:39 am Dharma dattu, <dharm...@gmail.com> wrote:
Hello All,
We have a job with 30 degree single bevel corner joint, as per client requirement we are using SAW process to complete on time schedule.
the fact is for root run the slag is not easy to be removed, as its hard and taking a lot of time even for grinding wheel / chipping. can some one say the reason for it. or a solution. 
Subsequent layers  slag is releasing on it's own, so i don't doubt filler metal or flux.
we are at present using base metal 20mm thk and 4mm filler metal, brand, D&H.

Regards,
Dharma Dattu. B

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.

Kannayeram Gnanapandithan

unread,
Dec 16, 2019, 5:08:43 AM12/16/19
to materials-welding
pl check any possibility of root by solid wire and further by saw
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/114d46f7-82a7-45a2-a8a7-41e1c67d5009%40googlegroups.com.

Devalkumar Desai

unread,
Dec 16, 2019, 10:24:37 PM12/16/19
to material...@googlegroups.com
You can use GTAW for root run and then continue with SAW for remaining welding


Amitabh Bhattacharya

unread,
Dec 19, 2019, 2:36:23 AM12/19/19
to material...@googlegroups.com
Hi Dharma,
Problem experienced  is typical to narrow V-groove SAW process. You haven't indicated base material in your mail. .

For SS/DSS base material ,SAW slag removal after root run is extremely difficult even with C-Steel.  

Following are suggestions for improvement:  

1) Joint design may be changed to U- groove with radius -use 6mm radius ball end mill.
2) Re-dry flux  250 deg F/2-3hrs on drying tray spead evenly even for new bag.
3) Root run by other process ( e.g GTAW) as suggested.

Hope this helps ...
Regards
Amitabh .