we have qualified a PQR (groove weld) for clad material (SA 240 410S (Clad) to Carbon Steel that is P7 to P1 material) using ER 309L Mo for the clad portion and E7018 for the rest.

Now we have to weld SA240 410S to SA240 410 S material for another job.

My question is, can we use the above said qualified PQR to make a wps of SA240 410S to SA240 410 S material, as other variables are same.

Thanking you,

Hareesh K V
+91-9447625012


pgoswami

unread,
Jun 13, 2016, 11:58:42 PM6/13/16
to material...@googlegroups.com

Hello Harish,

 

You require a separate PQR for clad plate welding. Look through ASME Sec-IX. It will tell you the differences between welding techniques and requirements of clad  welding and Non-cladded construction.

If there’s a qualified PQR for Carbon Steel welding that may be referred for welding the C.S part of the cladded   construction.

 

For 410s clad restoration one should qualify an overlay PQR.

 

Thanks.

 

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist

Ontario,Canada.

 


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAM3LgAVu5WdYUooGcah4gsV5LR3F8z9Se8JLoNnJgaGZE9hmFw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Lalu Rajendran

unread,
Jun 14, 2016, 2:43:53 AM6/14/16
to material...@googlegroups.com
Hi,

No, You must qualify a separate PQR for P7 to P7 with ER 309LMo.

regards,
LALU

makrand sakpal

unread,
Jun 14, 2016, 11:24:01 PM6/14/16
to material...@googlegroups.com

Is there any specific reason?

Kannayeram Gnanapandithan

unread,
Jun 15, 2016, 3:20:20 AM6/15/16
to materials-welding
change in Pno is essential variable.

For P7toP7, why 309L?

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

Lalu Rajendran

unread,
Jun 15, 2016, 7:01:39 AM6/15/16
to material...@googlegroups.com
Austenitic consumables (E309L) can be used for SS 410S material for temperature below 600 deg C due to sigma formation (Brittle phase) in the welds. Also PWHT can be avoided if you use E309L.

regards,
LALU 

Kannayeram Gnanapandithan

unread,
Jun 15, 2016, 11:14:46 PM6/15/16
to materials-welding

Lalu Rajendran

unread,
Jun 16, 2016, 12:55:15 AM6/16/16
to material...@googlegroups.com
​Yield value of 410S is 30 ksi​. 

Hareesh K V

unread,
Jun 16, 2016, 11:59:28 PM6/16/16
to materials-welding

Dear Sir,
There is no change in P No.
Please give me the reason with reference to ASME BPVC Sec IX.

Regards,

Hareesh K V

Raghuram Bathula

unread,
Jun 17, 2016, 12:12:51 AM6/17/16
to Materials-Welding
what is your qulaified PQR weld sequence? i guess weld the P1 material first and clad restoration on top it
do u need new WPS for clad restoration or groove weld? any way either case you need to qualify new PQR

George Dilintas

unread,
Jun 21, 2016, 10:26:13 PM6/21/16
to Meghanadh K
according to qw-403.11 and qw-424 you need a new pqr

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAM3LgAVu5WdYUooGcah4gsV5LR3F8z9Se8JLoNnJgaGZE9hmFw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis
Reply all
Reply to author
Forward
0 new messages