E 7018 or E 7018-1

98 views
Skip to first unread message

williams p wilson

unread,
Nov 2, 2022, 11:19:24 PM11/2/22
to material...@googlegroups.com
Dear Experts,
Greetings to all.

Could you please suggest suitable SMAW welding electrode (E 7018 or E 7018-1) for the below specifications,

MOC                                                   : SA 516 Gr.70 + N , 70 mm Thickness
PWHT                                                 :  610 ° C x 300 minutes minimum
Impact Test after HT                             :  -29° C
Weld Metal & HAZ Hardness (Max.) : 22 HRC

Thank You & Regards
Williams P Wilson
QA/QC Engineer
Please consider the environment before printing this message

Kannayeram Gnanapandithan

unread,
Nov 2, 2022, 11:47:33 PM11/2/22
to material...@googlegroups.com
go with E7018-1.
Even after SR, tensile will match with base metal. when sr is being done, in weldmetal 35Mpa is being reduced. Since 7018-1 has got more Manganese, it will will compensate the strength as well as impact also.
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHBxnQ54pJFzsM7_C_vd8EQ80eXy86A9CP38Kbh3%2BKKNHaJKyQ%40mail.gmail.com.

Vishwas Keskar Welding Manager WELDING

unread,
Nov 2, 2022, 11:54:23 PM11/2/22
to Materials & Welding
E7018 shall satisfy the requirement.
Pl ensure that the electrode batch is tested for  above   conditions mentioned by you .
Get the Welding Consumable Manufacturers confirmation .

Thanks 

Vishwas -IWE
International Welding Engineer

sujit kumar

unread,
Nov 3, 2022, 12:17:31 AM11/3/22
to material...@googlegroups.com
E-7018 Elextrode is acceptable for SA516 Gr 70 

Plese, ensure the electrode should be impact tested at -29 degrees. It will be available in MTC of the electrode.



Best Regards
Sujit kumar.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

james gerald

unread,
Nov 3, 2022, 1:32:32 AM11/3/22
to material...@googlegroups.com
Job thickness will give the requirement of Impact test if applicable.

Thanks & Regards

J.Gerald Jayakumar



james gerald

unread,
Nov 3, 2022, 3:51:18 AM11/3/22
to 'james gerald' via Materials & Welding
Job thickness of 70mm requires Impact test

Kannayeram Gnanapandithan

unread,
Nov 3, 2022, 4:30:07 AM11/3/22
to material...@googlegroups.com
image.png




pl see A6.4,  A 6.5.1 & 6.5.2

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349