Repair WPs

112 views
Skip to first unread message

udaya bhaskar

unread,
Dec 2, 2020, 10:30:19 PM12/2/20
to material...@googlegroups.com
Dear Giants,

I want to know about little doubt on piping welding repair WPS.
WPS made with 6010 and 7010 electrodes for regular welding.
Now I can plan with  6010 and 7018 electrodes for Repair WPS on the same .
Material :API5L PSL2 grade P1G1
is it allowable?
please correct me.
--
With Regards

Udaya bahaskar.D

Jamie Reyes

unread,
Dec 3, 2020, 12:58:28 AM12/3/20
to material...@googlegroups.com
If no impacts are involved, then yes. If I’m understanding you correctly, that is.....

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANii3RM0cJ%3DZOxjEpLzSnLu-ujsbFjpP4pYz71G-D9VXHwwC6A%40mail.gmail.com.
--
Regards,
Jamie Reyes
J.R. Machine Company, Inc.

Kannayeram Gnanapandithan

unread,
Dec 3, 2020, 1:33:30 AM12/3/20
to materials-welding
u can not use 7018 in place of 7010  because Fno is different which is an essential variable.

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


venkat chikkala

unread,
Dec 3, 2020, 2:28:27 AM12/3/20
to material...@googlegroups.com
Dear, 

You can use E6010 & E7018 for preparation of New WPS for repair, if project specification is silent about selection of electrode.

But existing WPS shall not be used with this combination of electrodes.

Regards,
CH V RAMANA 

Jamie Reyes

unread,
Dec 3, 2020, 2:28:27 AM12/3/20
to material...@googlegroups.com
Can you weld repair 7010 with 7018? Yes, With a PQR that is qualified per F4 Electrode,  along with all other essential variables. Kannayeram is correct. Hope this clears up any confusion.

udaya bhaskar

unread,
Dec 3, 2020, 2:28:28 AM12/3/20
to material...@googlegroups.com
Thank you for your advice.
But as per API1104 both F number is A5.5 . 
Table 1—Filler Metal Groups
image.png

Kannayeram Gnanapandithan

unread,
Dec 3, 2020, 6:37:16 AM12/3/20
to materials-welding
7010 comes under Group no 1 whereas  7018 comes under Group no 3.  Hydrogen level is more in 7010 than 7018

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Thu, Dec 3, 2020 at 2:30 PM Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote:
see the group no, no sfano. SFA no is not essential, only Group no or Fno as per ASME

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

Kannayeram Gnanapandithan

unread,
Dec 3, 2020, 6:37:17 AM12/3/20
to materials-welding
see the group no, no sfano. SFA no is not essential, only Group no or Fno as per ASME
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

Mohan q8

unread,
Dec 3, 2020, 6:37:31 AM12/3/20
to materials-welding
Dear, 

Pls clarify that your construction code is Piping of Pipeline?

For Pipeline and as per API 1104 you need to have qualified Repair WPS for repair. 



--
With Regards,

Mohan, Q8.

TDK YOKESH

unread,
Dec 13, 2020, 11:02:19 PM12/13/20
to material...@googlegroups.com
7010 you must be doing downhill and 7018 uphill progression. So your progression will change. 