As Per ASME Sec VIII, appendix R preheat criteria are determined for different PNumbers. 
But in case of welding of one BM from PNumber A to PNumber B, how can we determine the preheat criteria (temperature and thickness)?

Thanks,

Vishwas Keskar

unread,
Feb 24, 2021, 4:47:21 AM2/24/21
to material...@googlegroups.com
Apply the rules applicable for Higher P.No. of the two materials  being welded.
P no 4 to P No 5A _ Apply criteria for P NO 5A materilas.  Also consider pre heating addresed in WPS 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CABtwbJGO7XdR27uA9Lf9%3DQF_Wj%3Dd8daCV18xeQ7_OrsCT8u%2BVQ%40mail.gmail.com.

ishwar kumar

unread,
Feb 24, 2021, 4:47:24 AM2/24/21
to material...@googlegroups.com
Plz refer non mandatory appendix R 


--
IMG_20210224_095548.jpg

Sankaran Sp

unread,
Feb 24, 2021, 10:15:18 PM2/24/21
to material...@googlegroups.com
Dear friend,

when ever joining of two different P nos ( 5A+4) welding, following points to be  taken care :
1, Pre heating temp shall be maintained as higher Pno ( 5A)
2, PWHT  temp shall be maintained as per higher Pno(5A)
3, Consumable shall be maintained as per lower Pno( 4)




Regards,
Sankaran.SP
Welding & Metallurgy expert.


james gerald

unread,
Feb 25, 2021, 2:59:53 AM2/25/21
to 'Sankaran Sp' via Materials & Welding
Inline image


Inline image

Inline image

PWHT depends on condition and the selection of suitable welding consumable may be higher or lower P.No. It also depends on the P.No lower critical temperature and Tempering temperature and select buttering with Nickel consumable.

Thanks & Regards

J.Gerald Jayakumar



Kannayeram Gnanapandithan

unread,
Feb 25, 2021, 10:24:24 PM2/25/21
to materials-welding
Is it not recommended to use higher side also

Reply all
Reply to author
Forward
0 new messages