Dear experts,
We are going to start pqr for low alloy steels i.e. A335 Gr P11, P22, P5, P91 etc, it suppose to be post weld heat treated immediately after welding. As per literature if pwht is not possible immediately after welding, intermediate PWHT recommende .i.e pos heating.
Now the question is is there any code reference for the same? What is the heating time n temp???
The codes we r following here are shell dep's n asme b 31.3
Project: refinery
Awaiting for your reply
Thanks n regards
Prasad
0096594122634
U should not take it immediately for P91, it has to cool down below 100deg
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKgcArQMULX%3DQgcoXb8CgGM%3DmHiLQZG50iXgWuCR146W_HjO_g%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
What‘re thickness involved. You’ve to respect the materials engineering requirements, otherwise pay the price. For example it’s not advisable to weld P-91 steel without any provision for immediate PWHT. Better try when you’re ready with PWHT facilities.
You may delay PWHT for the other grade by adopting Post Heating or DHT, but may not have much luck with Garde-91 steel.
For P-91 a DHT @ 300-350 Deg C / 4 hrs is recommended as an alternative. Mind you NON-heat treated hardness of grade-91 steel would be easily over 350 HV, hence any impact loading, rough handling could crack the welds. Hence sooner the PWHT done, it’s better.
Also note DHT for grade -91 steel must be done after cooling the steel to room temperature for the whole martensitic transformation to occur. DHT should follow next. Without this the creep properties would be bad.
It’s better to know the full details first.
Shell DEP’s are exhaustive , read thoroughly & you’ll have the answer.
Thanks.
Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions w.r.t.
applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups
"Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email
to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
What‘re thickness involved. You’ve to respect the materials engineering requirements, otherwise pay the price. For example it’s not advisable to weld P-91 steel without any provision for immediate PWHT. Better try when you’re ready with PWHT facilities.
You may delay PWHT for the other grade by adopting Post Heating or DHT, but may not have much luck with Garde-91 steel.
For P-91 a DHT @ 300-350 Deg C / 4 hrs is recommended as an alternative. Mind you NON-heat treated hardness of grade-91 steel would be easily over 350 HV, hence any impact loading, rough handling could crack the welds. Hence sooner the PWHT done, it’s better.
Also note DHT for grade -91 steel must be done after cooling the steel to room temperature for the whole martensitic transformation to occur. DHT should follow next. Without this the creep properties would be bad.
It’s better to know the full details first.
Shell DEP’s are exhaustive , read thoroughly & you’ll have the answer.
Thanks.
Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Prasu Cutie
Sent: Saturday, August 06, 2016 10:33 PM
To: materials-welding@googlegroups.com
Subject: [MW:25208] Reg. post heating for low alloy steels
Dear experts,
We are going to start pqr for low alloy steels i.e. A335 Gr P11, P22, P5, P91 etc, it suppose to be post weld heat treated immediately after welding. As per literature if pwht is not possible immediately after welding, intermediate PWHT recommende .i.e pos heating.
Now the question is is there any code reference for the same? What is the heating time n temp???
The codes we r following here are shell dep's n asme b 31.3
Project: refineryAwaiting for your reply
Thanks n regards
Prasad
0096594122634
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKgcArQMULX%3DQgcoXb8CgGM%3DmHiLQZG50iXgWuCR146W_HjO_g%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAYAAAAAAAAAOT5XfyRhstKvyeqQRSrfFXCgAAAEAAAAERVFSdS96lDmj52mtEsPMgBAAAAAA%3D%3D%40quickclic.net.
For more options, visit https://groups.google.com/d/optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKgcArQMULX%3DQgcoXb8CgGM%3DmHiLQZG50iXgWuCR146W_HjO_g%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
Preheat maintenance is slightly different from post heating( dehydration, hydrogen bake out). Preheat maintenance is a non essential variable. Post heating is generally good for lowalloy/Cr-Mo steel to avoid HICC.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40DHhhM8FHP7VbPzhtqBpPwHVh8BTJMb%2BVAuQ%2BXOiYEJgw%40mail.gmail.com.
Starts at around 400 and finish around 120
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40BH-_3_0Z%2Boc9948pTkW1kZxSTh4kNs-fGCVuz3g%2BNxWg%40mail.gmail.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eM6GBWazBdjfHZ25B_cEWsK4cxRQA_o8fnXOH1g1x3wBA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
Mr lintas , preheat maintenance is a non essential variable as per QW 250
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40BAji%2ByncfvWDMOUqZmJthYMrYHEBY7eEOJbL_XZ6VtOQ%40mail.gmail.com.